- Open Access
- Total Downloads : 334
- Authors : Raja V, Sornakumar T
- Paper ID : IJERTV3IS110810
- Volume & Issue : Volume 03, Issue 11 (November 2014)
- Published (First Online): 19-11-2014
- ISSN (Online) : 2278-0181
- Publisher Name : IJERT
- License: This work is licensed under a Creative Commons Attribution 4.0 International License
Punch Life Improvement in Cold Forging of Nut
Raja V1, Sornakumar T2
1 Assistant Professor, Department of Mechanical Engineering
2Professor, Department of Mechanical Engineering
Sri Ramakrishna Institute of Technology, Coimbatore, India Thiagarajar College of Engineering, Madurai, India
Abstract Almost all fastener manufacturing industries are using metal forming process to manufacture nuts and bolts. Most of their operations depend on tools such as punches and dies, hence maintaining tool life as much as maximum will increase the profit margin. Punch service life, which defined as the maximum number of products produced before it fails. This paper focused on methodology to improve the punch life in cold forging of nut. Production cost is one of the major concerns in cold forging industry. Punches will fracture during extrusion and upsetting process. The metallurgical investigation of fractured extrusion punches shows brittle mode of failure. The impact properties of punch materials need to evaluate to control the brittle fracture. It is important to note down that the impact strength increases with decreasing hardness. Hence by changing tempering temperature it is possible to change the hardness of the punch material.
Keywords Punch life, Cold forging, Impact strength, Hardness and Tempering temperature
-
INTRODUCTION
In cold forging process, there are five stages of metal forming operation required to produce a nut. In each stage there will be a formation on punch side and die side. So the transfer mechanism is required to rotate the workpiece 1800 at each intemediate stages. The Figure 1.1 shows the sequence of nut forging. The number at the top of the figure represents the stages or stations. At 0th stage the raw material (10 B 21) is cut off to 9.21mm length and 18 mm diameter to produce standared M12X1.75 nut. At 1st stage the free formation carried out on punch side and die side. And the transfer mechanism is required to change the side of the raw material. Finally at 5th stage, the required dimensioned nut has been produced except internal thread.
Figure1.1: Stages of nut forging
Out of 5 stages, the extrusion punch (3rd stage) has to extrude and upset the raw material to a specified dimension. Hence, this punch should properly heat treated and surface treated.
The life of extrusion punches is very low as compared to other punches. Table1.1 presents the approximate punch life (in terms of number of nuts produced) taken from the cold forging industry.
Table 1.1: Punch Life
Stages
Punch life (number of nuts produced /
punch)
1
130000
2
80000
3
25000
4
75000
5
75000
Hence the aim of this paper is to improve the life of 3rd station punches without increasing the punch production cost so much. There have been several literatures referenced to explore the importance of impact loading in cold forging tool materials.
The Cold forging process is characterized by high forming and a high impact on the tool; therefore, the materials that are selected for cold forging tools have to be of high strength and high toughness [12]. Y.Zhang et al [12] conducted strain controlled fatigue test on Cr-Mo-V matrix type HSS at room temperature. Ryuichiro Ebara [8] presented the paper on Fatigue crack initiation and propagation behavior of cold forging die steels with respect to steel hardness. M. Dubar et al [6] Conducted wear analysis on AISI M2, and concluded that the CVD coating provides better performance than the PVD coating. K.V. Sudhakar [5] analyzed the fractrographic microstructures for extrusion die punches. It was observed that the fracture toughness property of the material should be evaluated rather than evaluating the material property with hardness. Yi-Chi Lee, Fuh-Kuo Chen [4] investigated the fatigue life of cold forging tools with respect to change in hardness property of the material. The relationship between the tool material properties such that yield strength, fracture strength and material hardness were constructed for various tempering temperature.
The research gap identified that the effect of impact property in cold forging tools should be analyzed. In this study, the comparison between existing (AISI M2) and selected high speed tool steel (AISI M42) were investigated. The most of cold extrusion punches being fractured in brittle
nature. The Figure 1.2 presents the brittle fractured cold extrusion punches of material AISI M2 and their relative hardness in the range of 58-62 HRC.
10 mm
10 mm
Figure 1.2: Macro view of Brittle fractured Punches
-
PROBLEM FORMULATION
In total production of a forged product, around 30% of cost incurred for tool production. Hence, it is important to notice tool life while performing forging operation. The forging machine has the ability to produce 155 nuts / min, but frequent stoppages due to punch failure, the production rate reduced to 137 nuts / min. In the competitive environment the tool maker should produce punches at low cost, but without degrading its quality. In the current forging industry, the punch material AISI M2 is purchased at annealed state.
The chemical composition (wt %) of AISI M2 (Material A) is given in Table 2.1. In order to increase the hardness of the material, it is first hardened by heating the material to austenite state and then sudden cooling or quenching with nitrogen gas. After hardening, the material hardness obtained in the range of 64-66 HRC. In order to reduce the retained austenite and increase the ductility of punch material, the process of tempering is important to consider.
Table 2.1: Chemical Composition of AISI M2
C
Mn
Si
Cr
Ni
Mo
W
V
0.92
0.3
0.3
3.5
0.3
5.2
6.0
2.0
Hence it is important to select the materials having high toughness and high hardness and also consider the availability of that particular material for an industry. The red hardness of the punches is primarily due to the presence of tungsten (W), chromium (Cr), vanadium (V) and molybdenum (Mo) [5].
-
METHODOLOGY
The adopted methodology is to increase the production rate but without increasing the cost of the product. By selecting appropriate punch material and effective heat treatment provides better life.
3.1 Material Selection
The alternative punch material was selected from the available punch material as AISI M42 (Material B) against the conventional punch material AISI M2. This material has greater amount of cobalt, molybdenum and carbon than the conventional material. The chemical composition of material B is given in Table 3.1.
Table 3.1: Chemical Composition of AISI M42
C
Mn
Si
Cr
Ni
Mo
W
V
Co
1.08
0.21
0.18
4.03
0.3
9.72
1.64
1.06
7.59
Higher the content of molybdenum increases hot hardness,hardenability and toughness of the material. Cobalt content increases hot hardness and wear resistance of the material.
3.2. Experimental Setup
The Izod-impact test specimens have prepared for various tempering temperature [4]. The Figure 3.1 shows the impact test specimen. Top side of punch has been attached with punch holder, so this set up assumed as a cantilever, then the izod impact test had been selected for the analysis.
Before impact
After impact
Figure 3.1: Izod Impact Test Specimens (ASTM E23)
-
Tempering process
The samples further allowed for hardening and tempering processes. The hardening of AISI M2 has following stages,
First Preheating – 650oC Second preheating – 870 oC Third preheating – 1050 oC Austenising – 1200 oC
Quenching – Nitrogen
Izod impact strength (J)
And the hardening of AISI M42 material has the following stages,
First Preheating – 650oC Second preheating – 870 oC Austenising – 1180 oC
Quenching – Nitrogen
For both materials, during hardening, the transformation of Austenite-Pearlite-Martensite [4] is required. The tempering temperature for material A is 530 – 570 oC. Hence, the range of tempering temperature was set to 200 – 700 oC for both the materials. To control retained austenite and increase ductility
60 55
14
12
10
8
6
4
2
0
50 45 40 35
Material A Material B
of the material, 3cycle tempering has been followed. The soaking time at every cycle set as 30min [4].
-
Hardness Test
Hardness test was done by using Digital Rockwell hardness tester (RASN-E) with Diamond ball indenter of
150 kg (hardened tool steels C scale). This hardness is taken at three different surfaces of the impact test specimen and the precision value has been taken for the further analysis. The results were plotted in the graph, and the Figure 3.2 represents the hardness value against the varying tempering temperature.
70
Hardness (HRC)
65
60
55
Hardness (HRC)
Figure 3.4: Izod impact strength Vs Hardness
The above graph shows that the effect of izod-impact strength for varying hardness of the punch material. Both Material A and Material B were increasing with increasing hardness. At the same time, the material B having greater amount of absorbed energy for the same hardness achieved in material A. hence Material B (AISI M42) is selected as a best alternative punch material as compared to Material A (AISI M2).
3.6 Microstructure
Microstructure analysis had been taken from metallurgical
50
45
40
35
200 300 400 500 600 700
Tempering Temp(oC)
Material A Material B
microscope. Fig 3.5 shows microstructures of material B at 200,500, 600 and 700oC.
Figure 3.2: Hardness Vs Tempering Temperature
-
Impact Test
The impact test has been taken out in Izod-impact Testing Machine (300N). The samples of at different tempering temperature are prepared for the impact test. At each temperature two samples were taken and their average impact strength (Joules) is taken and plotted in the Figure 3.3.
Impact strength (joules)
14
12
Ib = 1.691x + 1.013
10
8
6
Ia = 1.394x – 0.413
4
2
Material A Material B
0
200
Tem300perin4g00temp50e0ratur6e00 oC
700
Figure 3.3: Impact strength Vs Tempering temperature
From the results, observed that the impact strength of the material B is higher than material A for the same tempering temperature. Impact strength is determined from the amount of energy required to fracture specimen. The Figure 3.4 represents the effect of izod-impact value changes over changing the hardness value by varying the tempering temperature.
Figure 3.5: Microstructure of AISI M42
The correct temperature for material A was found as 550- 570oC. At 700 oC, the structure becomes carbon growing; hence this effect leads to decrease the hardness property of the material. By analyzing its microstructure, it was found that the temperature between 500-600oC becomes best structure. The even distribution of carbon and iron in martensite provides better strength to the material.
-
-
RESULTS
For molybdenum based tool steels (M-type), the tempering temperature ranges from 550-590oC becomes best combination of hardness and microstructure. Table 4.1 shows punch life for different trials.
Table 4.1: Punch Life at Different Trials
Table 4.2: Cost Estimation
Particulars
Material A
Material B
Material Cost (Rs)
750×0.28 = 210
1500×0.28= 420
Machining Cost (Rs)
220
220
Heat Treatment Cost (Rs)
77
77
CVD (Rs)
308
308
Polishing Cost (Rs)
120
120
Total Cost / Punch(Rs)
935
1145
The total cost for preparing Material A is Rs.935 and for Material B is Rs.1145. Punch producing cost for Material B is increased to 22.45% compared to Material A. Hence an extra cost required for material B is 210 / punch. Eventhough the material cost is increased for material B is compensated and advandageous when comparing the punch replacement cost. Table 4.3 presents the effect of punch replacement cost.
Table 4.3: Cost Savings
Particulars
Material A
Material B
Cost/Installation (Rs)
935
1145
No. of Replacements/day
12
4
Total installation Cost/day (Rs)
11220
4580
Total Savings/day (Rs)
–
6640
Due to failure occurred in third station punche, the number of replacing and installing new punches has been increasing daily. If the 3rd station punches replaced for every 20000 pieces, then for 1 shift, it should be replaced 12 times daily. Due to this problem, the change in installation after every failure increases operators fatigue.
For material A = 12 punches / day For material B = 4 punches / day
The absorbed impact energy is more for material B compared to material A. Hence material Bs replacement cost decreases and the total savings increases. Then, the operator fatigue decreased and the scrap due to punch failure were decreased.
Trial 1
Trial 2
Trial 3
Tempering Temp oC
520
550
570
Hardness HRC
62.964.8
65.6 66
63.4 65.2
Punch 1
31256
62675
42651
Punch 2
27805
67893
46547
Punch 3
25729
63543
39265
Average Punch Life
28263
64703
42812
Particulars
Material A
Material B
Production Rate / min
137
144
Production Quantity / day
197280
207360
Increased Production Quantity
/day
–
10080
Table 4.4: Production Rate Comparison
The total cost incurred for proucing punches including material cost, machining cost, heat treatment cost, CVD coating cost and polishing cost. Table 4.2 presents the various cost incurred for producing punches.
Material cost = Raw material cost (Rs) / Kg X Material
Weight (Kg) For material A = 750 x 0.28 = Rs 210
For material B = 1500 x 0.28 = Rs 420
By replacing the material A with material B the prodction quantity is increased. The rate at which the productionincreases is given as,
% rate of production increased / day = 5.11 %.
-
CONCLUSION
The fractured punches shows that the failure occurred due to inability to withstand impact strength. Hence, the material having high impact property had been selected and the material also checked for, in which hardness and tempering temperature the impact strength is higher for the material. The graph between impact strength Vs tempering
temperature and impact strength Vs hardness were presented. Then, the microstructure of selected punch material and the using material at different tempering temperature is given. The microstructure shows the optimum tempering temperature is lies between 500- 600oC. Then the test trials were conducted at these tempering temperatures. From the trial results, the material (AISI M42) hardness between 65.6-66 HRC gives better result compared with other trials and material A also. Therefore the tempering temperature for AISI M42 is kept at 550 oC gives better life. Production rate is increased by 5.11% per day. And, the cost savings by changing the material is obtained as Rs. 6640 per day.
REFERENCES
-
Yi-Che Lee, Fuh-Kho Chen, Failure analysis of a cold extrusion punches to enhance its quality and prolong its life, Journal of Material Processing Technology, 105 (2000)134-142.
-
Victor Vazquez, Daniel Hannan, Taylan Altan, Tool life in cold forging: an example of design improvement to increase service life Journal of Materials Processing Technology 98 (2000) 90-96.
-
M.L. Roessle, A. Fatemi, Strain-controlled fatigue properties of steels and some simple approximations International Journal of Fatigue 22 (2000) 495511.
-
Yi-Che Lee, Fuh-Kho Chen, Fatigue life of cold-forging dies with various values of hardness, Journal of Material Processing Technology, 113 (2001)539-543.
-
K.V. Sudhakar Micromechanics of fracture in extrusion die punch, Engineering Failure Analysis 9 (2002) 159165.
-
M. Dubar, A. Dubois, L. Dubar, Wear analysis of tools in cold forging: PVD versus CVD TiN coatings, Wear 259 (2005) 11091116.
-
G.H. Farrahi and H. Ghadbeigi, An investigation into the effect of various surface treatments on fatigue life of a tool steel Journal of Materials Processing Technology 174 (2006) 318324.
-
Ryuichiro Ebara, Fatigue crack initiation and propagation behavior of forging die steels International Journal of Fatigue 32 (2010) 830840.
-
A. R. Ab-Kadir, A. R. Othman, A. B. Abdullah, Mohd Riduan Ibrahim, Mohd Suyerdi, Prediction of Fatigue Life in Cold Forging Punch Design for Fastener Using Integrated FEA and Stress Life Approach
, Procedia Engineering, 50 ( 2012 ) 505 515.
-
S. Mitrovic, M. Babic, D. Adamovic,, F. Zivic, D. Dzunic, M. Pantic, Wear Behaviour of Hard Cr Coatings for Cold Forming Tools Under Dry Sliding Conditions, Tribology in Industry 34 (2012) 44-48.
-
X.G. Yan, D.Y. Li, Effects of the sub-zero treatment condition on microstructure, mechanical behavior and wear resistance of W9Mo3Cr4V high speed steel, Wear 302 (2012) 854-862.
-
Y. Zhang, C.L. Hu, Z. Zhao, A.P. Li, X.L. Xu Low cycle fatigue behaviour of a CrMoV matrix-type high-speed steel used for cold forging, Materials And Design 44(2013) 612-621.
-
S. Kalpakjian, Manufacturing Engineering and Technology, Third edition, 1985.