- Open Access
- Total Downloads : 537
- Authors : S.K.Chinta, Yogesh Wanere
- Paper ID : IJERTV1IS5291
- Volume & Issue : Volume 01, Issue 05 (July 2012)
- Published (First Online): 02-08-2012
- ISSN (Online) : 2278-0181
- Publisher Name : IJERT
- License: This work is licensed under a Creative Commons Attribution 4.0 International License
Practical Aspects Of Imparting Sun Protective Coating On Cotton Textiles
S.K.Chinta*, Yogesh Wanere
D.K.T.E.S.Textile & Engg. Institute, Ichalkaranji.
Abstract
The incidence of skin cancer has been rising for years worldwide. Elevated exposure to UV radiation is considering one of the main factors causing neoplasm of the skin. The risk to outdoors workers of exposure to solar ultraviolet radiation (UVR) has been known for some time. Textiles are a simple and effective means of protecting the skin against UV radiation. The UV protection depends on fiber type, yarn and fabric construction, square weight, moisture content, and finishing. To protect from any adverse affects due to exposure to ultraviolet light, a study was planned to provide protection for clothing using UVR absorbers. In the present study, cotton fabric in plain weave was coated with UV absorber by using titanium dioxide (TiO2), to develop sun protective textiles. The coating is carried out by using two different recipes by varying temperature and concentration. The coated fabrics were tested for
UPF testing using AATCC 183/2000 and AS/NZS:4399/1996 methods and also certain physical properties like crease recovery, bending modulus, crease recovery angle etc were tested using conventional procedures. The results indicated that the coating of TiO2 on cotton fabric improved the UV protection and also UPF values after washing do not alter noticeably.
Keywords: Ultraviolet Radiation (UVR), Titanium Dioxide (TiO2), Ultraviolet Protection Factor (UPF).
-
Introduction
Sunlight is the prime energy source and essential element for survival of human race. Sun radiation has a continuous energy spectrum over wavelength range of about 0.7 nm to 3000 nm and the effective spectrum of the solar radiation reaching on the surface of earth spans from 280 nm to 3000 nm [1], where the wavelength of ultraviolet spectrum lies between 290 nm to 400 nm. Ultraviolet radiation constitutes to 5% of the total incident sunlight on earth surface (visible light 50% and IR radiation 45%). Even though, its proportion is quite less, it has the highest quantum energy compared to other radiations. This energy of ultraviolet radiation is of the order of magnitude of bond energy of organic molecules; hence, it has tremendous detrimental effect on human skin [2, 3]. The intensity and distribution of ultraviolet radiation depends closely on the angle of incidence; hence they vary with the location of the place, season and time of the day. The incidence of skin cancer has been increasing at an alarming rate over the past several decades. Thought there are many factors involved in the onset of
melanoma and non-melanoma skin cancers, overexposure to ultraviolet radiation has clearly been identified as an important factor [4-6]. The long wavelength (320 nm-400 nm) ultraviolet rays (UV-
A) causes a transformation of melanin precursors in the skin, leading to so-called rapid pigmentation, which sets in within a period of a few hours, but this is only a very minimal and of short duration. However, it penetrates deeply into the dermis or true skin, leading to premature ageing, showing up in the form of loss of elasticity accompanied by lines and wrinkles. The shorter wavelength (290 nm-320 nm), but higher energy ultraviolet rays (UV-B) penetrate to a depth of a few millimeters into the skin, causing the formation of a relatively stable pigment in the cells of the outer layer of the skin. This can lead to acute chronic reactions and damages; such as skin reddening (erythema) or sunburn. The shortest wavelength (10 nm-290nm) ultraviolet rays (UV-C), which are highly damaging to human skin are filtered out by the ozone layer and do not reach on the surface of earth [7-11].
The risks posed by ultraviolet radiation have become more dangerous in recent years as the whole world is suffering from all kinds of pollution. Clothing has the ability to protect the skin from incident solar radiation because the fabric from which it is made can reflect, absorb and scatter solar wavelengths. Each fabric must be tested to determine its ability to protect from solar radiation, as this cannot be known from visual observation nor calculated from descriptions of the fabrics composition and structure. To determine this so called Ultraviolet Protection Factor (UPF), special test standards and methods are required as offered by different associations. Care labeling similar to fabric and garment care labels has
been developed for UV protection, and standard procedures have been established for the measurement, calculation, labeling methods and comparison of label values. [12]
Ultraviolet Protective Factor Ratings [7]
UVR
Protection Category
UV
Protection Factor
Mean %UVR Transmission
Moderate
UPF 10 to 19
10 to 5.1
High
UPF 20 to 29
5.0 to 3.4
Very High
UPF 30 to 49
3.3 to 2.0
Maximum
UPF
50
2.0
Thus in this study, coating of titanium dioxide (TiO2) was carried out on plain woven cotton fabric, using two different recipes by varying temperature and concentration. The UPF of coated samples were measured by using AATCC 183/2000 and AS/NZS: 4399/1996 methods.
-
Material and methods
-
Fabric
For this study 100% cotton plain woven shirting fabric was used.
30sx30s
——— 82
106 × 106
GSM 140 gm/sq mtr, Thickness 0.29mm.
-
Pretreatment of fabric
The raw fabric was desized by using enzyme desizing then scouring was carried out at boil temperature for 4hrs. After that bleaching is carried out using 4% H2O2 of 50% concentration for 4hrs followed by H2O2 killer, the fabric is then washed and dried.
-
Fabric Treatment: coating of fabric with titanium dioxide (TiO2)
-
The cotton fabric was coated with titanium dioxide as UV absorber by using three different concentration (1%, 2%, and 4%) gpl and two different recipes.
Coating recipes of titanium dioxide for cotton fabric. Recipe A:
UV absorber TiO2 – (1%, 2%, 4%) gpl
Ammonium sulphate – 1.0 gpl
Formic acid – 1.0 gpl
Synthetic thickener – as per requirement
Recipe B:
UV absorber TiO2 – (1%, 2%, 4%) gpl
Sodium bicarbonate – 4 gpl
Urea – 60 gpl
Synthetic thickener – as per requirement
The coating was carried out on Mathis Continuous Coating Mathis Type KTF-S-500. The fabric was
then dried at 800c for 2min and curing was carried out at three different temperatures, i.e. at 1200c, 1400c and 1600c for 4min.
-
Testing
-
Determination of UPF of fabric samples [13]
The UPF of fabric samples were tested by using standard AATCC 183/2000 and AS/NZS: 4399/1996 on Spectrophotometer.
-
UPF after Washing [14]
For washing treatment the 5gpl soap solution was used and washed in launder Ometer meter machine for 90 min at 400c and then check the UPF values of washing samples were checked by using standard AS/NZS: 4399/1996.
-
Tearing strength [15]
Fabric samples were evaluated for tearing strength on tearing tester as per the IS 6359:1971SP-15 the test specimen was according to template.
-
Bending Modulus [16]
Fabric samples were evaluated for Bending Modulus on stiffness tester as per the IS 659:1971SP-15 methods, the test specimen was according to template.
-
Crease recovery angle [15]
-
Fabric samples were evaluated for Crease recovery angle on Crease recovery tester as per the IS 6359:1971SP-15 methods, the test specimen was according to template.
2. Results and Discussion
Recipe-A
Table 1:- Effect of temperature and concentration of recipe-A on UPF values
Values of UPF |
|||||||||
120 0C |
140 0C |
160 0C |
|||||||
1 |
2 |
4 |
1 |
2 |
4 |
1 |
2 |
4 |
|
g/l |
g/l |
g/l |
g/l |
g/l |
g/l |
g/l |
g/l |
g/l |
|
UPF |
26 |
32 |
41 |
27 |
34 |
43 |
29 |
35 |
45 |
valu |
2. |
5. |
0. |
6. |
1. |
3. |
0. |
9. |
5. |
es |
81 |
19 |
54 |
18 |
22 |
16 |
72 |
23 |
39 |
UPF values
600
400
200
0
g/lg/lg/lg/lg/lg/lg/lg/lg/l
UPF values
1 2 4 1 2 4 1 2 4
Graph 1:- Effect of temperature and concentration of recipe-A on UPF values
Results of Table 1 and Graph 1 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of UPF also increases from 262.81 to
410.54 respectively. As the temperature of curing increases from 1200c to 1600c, the trend of UPF is of
increasing order and the maximum UPF value was found to be 455.39 for 4gpl TiO2 concentration at 1600c. The increase in UPF values may be due to the presence TiO2 which reduced the UV transmission. Also increasing the curing temperature may attribute to higher cross linking efficiency of coated fabrics.
Table 2:- Effect of temperature and concentration of recipe-A on values of UPF after washing
Values of UPF after washing |
||||||||||
120 0C |
140 0C |
160 0C |
||||||||
1 |
2 |
4 |
1 |
2 |
4 |
1 |
2 |
4 |
||
g/ l |
g/ l |
g/ l |
g/ l |
g/ l |
g/ l |
g/ l |
g/ l |
g/ l |
||
2 |
3 |
4 |
2 |
3 |
4 |
2 |
3 |
4 |
||
6 |
2 |
1 |
7 |
4 |
3 |
9 |
5 |
5 |
||
UPF of |
2. |
5. |
0. |
6. |
1. |
3. |
0. |
9. |
5. |
|
coated |
8 |
1 |
5 |
1 |
2 |
1 |
7 |
2 |
3 |
|
fabric |
1 |
9 |
4 |
8 |
2 |
6 |
2 |
3 |
9 |
|
2 |
2 |
3 |
2 |
2 |
3 |
2 |
3 |
3 |
||
UPF |
2 |
7 |
4 |
3 |
9 |
7 |
5 |
0 |
9 |
|
after |
6. |
9. |
0. |
7. |
2. |
0. |
0. |
9. |
1 |
|
washin |
1 |
5 |
3 |
3 |
7 |
1 |
2 |
1 |
||
g |
8 |
6 |
6 |
8 |
6 |
1 |
||||
1 |
1 |
1 |
1 |
1 |
1 |
1 |
||||
3. |
4. |
1 |
4. |
1 |
4. |
3. |
3. |
4. |
||
% |
9 |
0 |
7. |
0 |
4. |
5 |
9 |
9 |
1 |
|
change |
3 |
5 |
1 |
5 |
2 |
3 |
1 |
5 |
3 |
534200
g/l g/l g/l g/l g/l
1 2 4 1 2 4 1 2 4
120 0C 140 0C 160 0C
UPF of coated
fabric
UPF after washing
% change
Values of UPF after
washing
100
Graph 2:- Effect of temperature and concentration of recipe-A on values of UPF after washing
Results of Table 2 and Graph 2 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of UPF after washing increases from
226.18 to 340.3 respectively. As the temperature of curing increases from 1200c to 1600c, the trend of values of UPF after washing are of increasing order and the maximum UPF value was found to be 391.0 respectively for 4gpl TiO2 concentration at 1600c. The UPF value was found to be decreased up to 14.53% after application. UPF values before and after indicates average reduction in UPF of about 14% which indicates the stability of the coating during washing. The reason behind this may be higher cross linking efficiency.
Table 3:- Effect of temperature and concentration of recipe-A on tearing strength values
un- treat ed sam ple |
Values of Tearing strength(gram force) |
|||||||||
120 0C |
140 0C |
160 0C |
||||||||
1 |
2 |
4 |
1 |
2 |
4 |
1 |
2 |
4 |
||
g / l |
g/ l |
g /l |
g /l |
g/ l |
g/ l |
g/ l |
g/ l |
g /l |
||
warp (gf) |
141 8.66 |
1 3 8 0 |
1 3 1 2. 6 6 |
1 2 2 6 |
1 3 6 0 |
1 2 9 0. 3 3 |
1 1 9 4. 3 3 |
1 2 6 2. 6 6 |
1 2 2 6. 6 6 |
1 0 8 8 |
Weft (gf) |
928 |
8 9 6 |
8 6 4 |
8 5 3 . 3 |
8 8 5 . 3 3 |
8 3 8 |
7 8 4 |
8 4 8 |
8 0 0 |
7 5 5 |
% chan ge in warp |
2 . 7 2 |
7. 4 7 |
1 3 . 5 8 |
4 . 1 3 |
9. 0 4 |
1 5. 8 1 |
1 3. 5 3 |
1 0. 9 9 |
2 3 . 3 |
|
% chan ge in weft |
3 . 4 4 |
6. 8 9 |
8 . 0 4 |
4 . 5 9 |
9. 6 9 |
1 5. 5 1 |
8. 6 2 |
1 3. 7 9 |
1 8 . 6 4 |
1500
1000
500
0
g/l g/l g/l g/l 1 2 4 1 2 4 1 2 4
120 0C 140 0C 160 0C
warp (gf) Weft (gf)
% change in warp
Graph 3: – Effect of temperature and concentration of recipe-A on tearing strength values
Results of Table 3 and Graph 3 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of tearing strength (in gram force) decreases from 1380 to 1226 and 896 to 853.33 in both warp and weft directions respectively. As the temperature of curing increased from 1200c to 1600c, the trend of tearing strength values were of decreasing order and the minimum tearing strength (in gram force) values were found to be 1088 and 755 in both warp and weft directions respectively for 4gpl TiO2 concentration at 1600c. The tearing strength values were found to be decreased by 23.30% and 18.64% respectively after application. The reason may be attribute to the cross linking efficiency. More the cross linking more will be reduction in strength.
Table 4:- Effect of temperature and concentration of recipe-A on values of bending modulus
Un- treat ed sam ple |
Values of Bending modulus |
|||||||||
120 0C |
140 0C |
160 0C |
||||||||
1 |
2 |
4 |
1 |
2 |
4 |
1 |
2 |
4 |
||
g /l |
g / l |
g/ l |
g /l |
g/ l |
g/ l |
g/ l |
g/ l |
g/ l |
||
Be nd in g m od ul us |
54 |
9 3. 0 6 |
1 0 4 |
1 5 7. 8 8 |
9 4. 4 5 |
1 0 5. 3 4 |
1 6 2. 4 4 |
1 0 5. 1 7 |
1 3 3. 8 2 |
1 7 1. 5 8 |
g/l 1 |
g/l 2 |
g/l 4 |
g/l 1 |
g/l 2 |
g/l 4 |
g/l 1 |
g/l 2 |
g/l 4 |
200
100
0
Bending modulus
Bending
modulus
Graph 4:- Effect of temperature and concentration of recipe-A on values of Bending modulus
Results of Table 4 and Graph 4 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of bending modulus increases from 93.06
to 157.88 respectively. As the temperature of curing increases from 1200c to 1600c, the trend of Bending modulus values were of increasing order and the maximum Bending modulus value was found to be
171 respectively for 4gpl TiO2 concentration at 1600c.
Table 5:- Effect of temperature and concentration of recipe-A on values of Crease recovery angle
Un- treated sample |
Values of Crease recovery angle |
|||||||||
120 0C |
140 0C |
160 0C |
||||||||
1 g/ l |
2 g/ l |
4 g /l |
1 g /l |
2 g /l |
4 g /l |
1 g /l |
2 g /l |
4 g /l |
||
W arp |
105 |
9 8 |
9 4 |
8 8 |
9 5 |
9 1 |
8 7 |
8 5 |
8 0 |
7 6 |
W eft |
111 |
1 0 6 |
1 0 1 |
9 6 |
9 8 |
9 2 |
8 5 |
8 0 |
8 2 |
7 8 |
120
100
80
60
40
20
0
g/l g/l g/l g/l g/l g/l g/l g/l g/l 1 2 4 1 2 4 1 2 4
120 0C 140 0C 160 0C
Warp Weft
Graph 5: – Effect of temperature and concentration of recipe-A on values of Crease recovery angle
Results of Table 4 and Graph 4 indicate that as concentration of TiO2 increases from 1gpl to 4gpl, the values of Crease recovery angle decreases from
-
to 88 and 106 to 96 in both warp and weft directions respectively. As the temperature of curing increased from 1200c to 1600c, the trend of Crease recovery angle values are of decreasing order and the minimum Crease recovery angle values were found to be 76 and 78 in warp and weft directions respectively for 4gpl TiO2 concentration at 1600c. The reduction in crease recovery angle may be due to stiffness of the fabric after coating and cross linking.
Recipe-B
Table 6:- Effect of temperature and concentration of recipe-B on UPF values
Values of UPF
120 0C
140 0C
160 0C
1
2
4
1
2
4
1
2
4
g/l
g/l
g/
l
g/l
g/l
g/l
g/l
g/l
g/l
UPF
valu es
15
9.
73
28
2.
44
3
1
7.
16
8.
15
29
7.
83
33
4.
42
17
6.
46
31
3.
14
35
5.
18
7
100
4320000
UPF values
g/lg/lg/lg/lg/lg/lg/lg/lg/l 1 2 4 1 2 4 1 2 4
120 0C 140 0C 160 0C
UPF values
Graph 6:- Effect of temperature and concentration of recipe-B on UPF values
Results of Table 6 and Graph 6 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of UPF also increases from 169.73 to
317.7 respectively. As the temperature of curing increases from 1200c to 1600c, the trend of UPF is of increasing order and the maximum UPF value was found to be 355.18 for 4gpl TiO2 concentration at 1600c. The increase in UPF values may be due to the presence TiO2 which reduced the UV transmission. Also increasing the curing temperature may attribute to higher cross linking efficiency of coated fabrics.
Table 7:- Effect of temperature and concentration of recipe-B on values of UPF after washing
Values of UPF after washing
120 0C
140 0C
160 0C
1
2
4
1
2
4
1
2
4
g/
l
g/
l
g/
l
g/
l
g/
l
g/
l
g/
l
g/
l
g/
l
1
2
3
1
2
3
1
3
3
5
8
1
6
9
3
7
1
5
UPF of
9.
2.
7.
8.
7.
4.
6.
3.
5.
coated
7
4
7
1
8
4
4
1
1
fabric
3
4
5
3
2
6
4
8
1
2
2
1
2
2
1
2
3
UPF
4
4
7
4
5
8
5
7
0
after
0.
2.
2.
6.
6.
7.
1.
0.
5.
washin
6
4
5
1
3
2
3
1
3
g
5
2
6
4
6
8
1
1
1
1
1
1
1
1
1.
4.
4.
3.
3.
1
4.
3.
4.
%
9
1
2
0
9
4.
2
7
0
change
7
5
2
7
4
1
2
1
4
2100
UPF of coated
g/l g/l g/l g/l g/l
1 2 4 1 2 4 1 2 4
fabric
UPF after washing
% change
120 0C 140 0C 160 0C
0
4300
Graph 7:- Effect of temperature and concentration of recipe-B on values of UPF after washing
Results of Table 7 and Graph 7 indicate that as concentration of TiO2 increases from 1gpl to 4gpl, the values of UPF after washing increases from 140.6 to 272.52 respectively. As the temperature of curing increases from 1200c to 1600c, the trend of values of UPF after washing are of increasing order and the maximum UPF value was found to be 305.3 respectively for 4gpl TiO2 concentration at 1600c. The UPF value was found to be decreased up to 14.22% after application. UPF values before and after indicates average reduction in UPF of about 14% which indicates the stability of the coating during washing. The reason behind this may be higher cross linking efficiency.
Table 8:- Effect of temperature and concentration of recipe-B on tearing strength values
un- treat ed sam ple
Values of Tearing strength(gram force)
120 0C
140 0C
160 0C
1
2
4
1
2
4
1
2
4
g/
l
g
/l
g/
l
g/
l
g
/l
g
/l
g
/l
g
/l
g
/l
warp (gf)
1418
.66
1
4
1
1.
2
5
1
3
7
6
1
3
3
3.
3
3
1
3
4
4
1
3
0
2
1
2
4
0
1
2
3
8
1
1
3
6
1
0
4
0
Weft (gf)
928
8
9
6
8
8
2
8
3
2
8
7
4.
8
3
2
7
6
8
8
1
6
7
8
4
7
5
2
6
6
%
0.
2
6.
5.
8
1
1
1
2
chan
5
.
0
2
.
2
2
9
6
ge in
1
4
1
6
2
.
.
.
.
warp
9
2
5
7
9
6
9
3
2
9
%
3
4
1
5
1
1
1
chan
.4
.
0.
.7
1
7
2
5
1
ge in
4
9
3
4
0
.
.
.
8
weft
5
4
.
2
0
5
.
3
4
6
1
9
4
6
12000
16400
4200
860000
0
g/lg/lg/lg/lg/lg/lg/lg/lg/l 1 2 4 1 2 4 1 2 4
120 0C 140 0C 160 0C
warp (gf) Weft (gf)
% change in warp
% change in
uVna-lturesatoefdTearing strength(gram force)weft
sample
Graph 8: – Effect of temperature and concentration of recipe-B on tearing strength values
Results of Table 8 and Graph 8 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of tearing strength decreases 1411.25 to
133.33 and 896 to 853.33 in both warp and weft
directions respectively. As the temperature of curing increases from 1200c to 1600c, the trend of tearing strength values are of decreasing order and the minimum tearing strength values were found to be 1088 and 755 in both warp and weft directions respectively for 4gpl TiO2 concentration at 1600c. The tearing strength values were found to be decreased by 26.69% and 18.96% respectively after application. The reason may be attribute to the cross linking efficiency. More the cross linking more will be reduction in strength.
Table 9:- Effect of temperature and concentration of recipe-B on values of Bending modulus
Un- treat ed samp le
Values of Bending modulus
120 0C
140 0C
160 0C
1
2
4
1
2
4
1
2
4
g
/ l
g/ l
g/ l
g/ l
g
/l
g/ l
g/ l
g/ l
g/ l
Ben ding mod ulus
54
9
4
1
1
2.
3
9
1
4
0.
7
9
1
0
8.
2
2
1
2
7
. 8
1
5
7.
2
4
1
3
8.
0
2
1
6
2.
0
3
1
9
9.
2
5
Bending modulus
2500
g/lg/lg/lg/lg/lg/lg/lg/lg/l
1 2 4 1 2 4 1 2 4
Bending
modulus
120 0C 140 0C 160 0C
Un- trVealtuedes of Bending modulus sample
50
1500
Graph 9:- Effect of temperature and concentration of recipe-B on values of Bending modulus
Results of Table 10 and Graph 10 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of bending modulus increases from 94 to 140.79 respectively. As the temperature of curing increases from 1200c to 1600c, the trend of Bending modulus values are of increasing order and the maximum Bending modulus value was found to be 199.25 respectively for 4gpl TiO2 concentration at 1600c.
Table 10:- Effect of temperature and concentration of recipe-B on values of Crease recovery angle
Un- treated sample
Values of Crease recovery angle
120 0C
140 0C
160 0C
1
2
4
1
2
4
1
2
4
g/
l
g/
l
g
/l
g
/l
g
/l
g
/l
g
/l
g
/l
g
/l
W
ar p
105
9
9
9
5
9
0
9
5
9
1
8
6
8
6
7
8
7
4
W
eft
111
1
0
6
1
0
0
9
4
9
9
9
5
8
9
8
3
7
8
7
5
120
100
80
60
40
20
0
g/l g/l g/l g/l g/l g/l g/l g/l g/l
Warp
Weft
1 2 4 1 2 4 1 2 4
120 0C 140 0C 160 0C
Graph 10: – Effect of temperature and concentration of recipe-B on values of Crease recovery angle
Results of Table 10 and Graph 10 indicate that as the concentration of TiO2 increases from 1gpl to 4gpl, the values of Crease recovery angle decreases from
-
to 90 and 106 to 94 in both warp and weft directions respectively. As the temperature of curing increases from 1200c to 1600c, the trend of Crease recovery angle values are of decreasing order and the minimum Crease recovery angle values were found to be 74 and 76 in warp and weft directions respectively for 4gpl TiO2 concentration at 1600c. The reduction in crease recovery angle may be due to stiffness of the fabric after coating and cross linking.
Conclusions
From the results and discussion it was found that
Due to the coating of TiO2 on cotton fabric, it increases UPF values. At 4% concentration and 1600c temperature, UPF value is higher.i.e.
455.39 of Recipe A.
Recipe-A provided better UPF values as compare to Recipe-B.
UPF values after washing reduced up to 14.33% in recipe-A and 14.22% in recipe-B and which indicates the durability of sun protective coating.
Recipe-A was found to be slightly better as against Recipe-B as far as tearing strength and bending modulus are concerned.
References:-
-
UV radiation protective clothing, available at http://www.benthamscience.com/open/totextilej/ articles/V003/14TOTEXTILEJ.pdf
-
F. Palacin, Textile finish protects against ultraviolet radiation, Melliand Int., vol. 3, pp. 169-172, 1997.
-
Akaydin, M., Research of UV Permeability Properties of Basic Weft Knitted Structures,
Scientific Research and Essays, 5, 2169-
2178(2010).
-
Kursun, S., and Ozcan G., Investigation of UV Protection of Swimwear Fabrics, Textile Research Journal, 80(17), 1811-1818(2010).
-
Saravanan, D., UV Protection Textile Materials, AUTEX Research journal, 7, 53-62(2007).
-
Saxen, A., and Srivastava, A., Sun Screen Shelter Fabric, Textile Review, 5, 16-21, (2010).
-
Menezes, E., UV Protective Finish, Man-Made Textile in India, 52, 59-61, (2009).
-
Pai, S. R., and Paul, R., UV Absorber and Their Importance In Industry, New Cloth Market, 18, 79-82(2003).
-
Bajaj, P., Kothari, V. K., and Gosh, S.B., Some Innovations in UV Protective Clothing, Indian Journal of Fibre and Textile Research, 25, 315- 329(2000).
-
Elhendawy, A. G., EL-Nagar, K., and EL- Ttahlawy, K., Cyclodextrin-4 Hydroxy Benzophenone Inclusion Complex for UV protective Cotton Fabric, Journal of Textile Institute, 98, 453-462, (2007).
-
Nishkam, A., Sahu, H. C., Gupta, k. k., and Kasturiya, N., Snow Camouflage, Man-Made Textile In India, 10, 402-408(2002).
-
Hussain, A., and Dr. Jahan, S., Protective Textiles: Protection Against UV Radiation, available at: www.fibre2fashion.com.
-
Richard A. Scott, Textile for Protection, first Edition, Woodhead publication , 2005.
-
Pradip V. Mehata and Satish K. Bhardwaj, Managimg Quality in the Apparel Industry, first Edition, New Age International(P), 1988.
-
B. P. Saville, physical Testing of Textile, first Edition, Woodhead publication, 1999.
-
J. E. Booth, Principle of Textile Testing, frist Edition, CBS publication, 1996.
*To whom the correspondence is made
Prof (Dr.) S.K. Chinta
Textile and Engineering Institute, D.K.T.E Rajwada, Ichalkaranji, Maharashtra