- Authors : Sumaya Beevi, Deepthi R Nath,
- Paper ID : IJERTCONV3IS29055
- Volume & Issue : NCRACE – 2015 (Volume 3 – Issue 29)
- Published (First Online): 30-07-2018
- ISSN (Online) : 2278-0181
- Publisher Name : IJERT
- License: This work is licensed under a Creative Commons Attribution 4.0 International License
Ultimate Strength Determination Due to Addition of Polypropylene Fibre in Optimum Replacement of Cement by GGBS
Sumaya Beevi
M. Tech Student,
Civil Engineering Department,
Younus College of Engineering and Technology, Kollam, Kerala, India
Deepthi R Nath,
Assistant Professor, Civil Engineering Department
Younus College of Engineering and Technology Kollam, Kerala, India
AbstractUsually Ordinary Portland Cement concrete is used for making the civil structures. Portland cement can be replaced by Ground Granulated Blast Furnace Slag (GGBS). The Ground granulated Blast furnace slag (GGBS) is an industrial waste and a pozzolanic material that has received considerable attention in both research and application. It is a by-product of the steel industry. GGBS is produced when molten slag is quenched rapidly using water jets, which produces a granular glassy aggregate. It is suitable for concrete mix and improves properties of concrete like compressive strength, workability etc .The present investigation has been undertaken to study the effect of Ground granulated blast furnace slag on the properties of concrete when cement is replaced by GGBS in different percentages varying from 0% to 60% at an interval of 10%.After getting the optimum replacement percentage polypropylene fibre is added in varying proportions such as 0%, 0.25%, 0.5%, 0.75% and 1%. The main objective of this study is to determine the optimum strength obtained by addition of polypropylene fibre to mix corresponding to optimum cement replacement by GGBS under the Indian conditions to satisfy the strength requirements.
KeywordsPolypropylene, GGBS, Shear strength
-
INTRODUCTION
OPC based concrete continues to be the pre-eminent construction materials for use in any type of civil engineering structures because of its easiness in construction, performance in strength requirements, better durability in normal environment, in comparison to other construction materials like steel, timber etc. At the same time some problems are also associated with this. At present the cement industries produced approximate 7% of total carbon dioxide produced in the world, which is very alarming to our protective Ozone layer. Second problem is the lower durability in aggressive environment. Use of mineral admixtures like Ground Granulated Blast Furnace Slag (GGBS), Silica Fume (SF), Fly Ash (FA) etc. in concrete may be the better solution in above conditions. These admixtures also offer benefits with respect to the cost of concrete.
A. Ground granulated blast furnace slag (GGBS)
Ground Granulated Blast Furnace Slag (GGBS) is a by- product of the steel industry. GGBS is produced when molten slag is quenched rapidly using water jets, which produces a granular glassy aggregate. Thus Ground Granulated Blast Furnace Slag is advantageous over various other cementing materials because of the following reasons:-
-
Non-hazardous and non-metallic waste of the Iron industry.
-
Eco-friendly and useful for construction work.
-
Helps to improve the properties of concrete like compressive strength, workability etc.
-
Low cost and easily available.
-
-
OBJECTIVE
Present experimental work explores the possibility of using GGBS as replacement of cement in concrete and polypropylene fibre to improve ductility. The main objective of this study is
-
To develop a proper mix proportion for normal concrete and GGBS modified concrete mix.
-
To study the workability and fresh concrete properties of normal concrete and GGBS modified concrete mix.
-
To study the mechanical properties of normal concrete and GGBS modified concrete mix.
-
To determine the optimum replacement percentage of GGBS modified concrete mix.
-
To determine the optimum percentage of polypropylene fibre in the above determined concrete mix.
-
-
EXPERIMENTAL INVESTIGATION
This chapter deals with the experimental programmes conducted in the present study which include material characterization, mix design, properties of fresh concrete and properties of hardened concrete. The main objective of the study is to investigate the impact of polypropylene fibre on the mechanical properties and ultimate strength of concrete with optimum replacement of cement by GGBS under standard conditions.
-
Constituent materials
Cement: Ordinary Portland cement of 53 grade confirming to IS 12269:1987 was used for the study. For the cement the standard consistency test, initial setting time test, final setting time test and specific gravity test were conducted. The standard consistency of cement used is 36.25%.
Fine aggregate: M sand is used as fine aggregate. Msand passing through 4.75mm IS sieve conforming to grading zone II of IS 383:1970 was used. Specific gravity and fineness modulus of Sand used were 2.4 and 2.87 respectively.
Coarse aggregate: Coarse aggregate of maximum size 20 mm from local source was used.
Ground Granulated Blast Furnace Slag: Different laboratory tests were conducted on GGBS to determine standard consistency, Fineness, Specific Gravity. The standard consistency of GGBS used is 35.55%. The chemical composition of GGBS as shown in table 1
TABLE 1 CHEMICAL COMPOSITION OF GGBS
Sl. No.
Chemical Composition
%Weight
1
Glass
85-98
2
Silica(SiO2)
17-38
3
Lime(CaO)
3.84
4
Iron Oxide
0.5-2
5
Magnesia(MgO)
4-17
6
Alumina
15-20
7
MnO2
1-5
Polypropylene Fibre: Polypropylene fibres of length 12mm was used for the study. Physical properties of polypropylene are given by the manufacturer as shown in table 2.
TABLE 2 PROPERTIES OF POLYPROPYLENE
Sl. No.
Properties
Values
1
Type of Fibre
Virgin Polypropylene Homo-Polymer
2
Length of Fibre (mm)
12
3
Diameter of Fibre (µm)
37.7
4
Aspect Ratio
318
5
Ultimate Tensile Strength(MPa)
550-600
6
Specific Gravity
0.91
Superplasticizer: In order to achieve the desired workability, poly carboxylate ether based new range water reducing admixture, Cera Hyperplast XRW40 was used as the superplasticizer. Cera Hyperplast XRW40 is available in liquid, which is dispensed into the concrete along with water.
Water: Potable water is generally considered as being acceptable.
Reinforcement: High Yield Strength Deformed Steel bars of 6 mm, 8 mm and 10mm diameter were used for the study.
-
Preliminary laboratory work
This work was done to find the optimum replacement of cement by GGBS.
Mix Designation
Description
Cube
Cylinder
Beam
GGBS0
0% cement replaced by GGBS
6
3
3
GGBS1
35% cement replaced by GGBS
6
3
3
GGBS2
40% cement replaced by GGBS
6
3
3
GGBS3
45% cement replaced by GGBS
6
3
3
GGBS4
50% cement replaced by GGBS
6
3
3
GGBS5
55% cement replaced by GGBS
6
3
3
GGBS6
60% cement replaced by GGBS
6
3
3
TOTAL
42
21
21
Mix Designation
Description
Cube
Cylinder
Beam
GGBS0
0% cement replaced by GGBS
6
3
3
GGBS1
35% cement replaced by GGBS
6
3
3
GGBS2
40% cement replaced by GGBS
6
3
3
GGBS3
45% cement replaced by GGBS
6
3
3
GGBS4
50% cement replaced by GGBS
6
3
3
GGBS5
55% cement replaced by GGBS
6
3
3
GGBS6
60% cement replaced by GGBS
6
3
3
TOTAL
42
21
21
TABLE 3 DETAILS OF SPECIMEN FOR GGBS MIXES
-
Tests on specimens
-
Compressive strength
-
TABLE 4 COMPRESSIVE STRENGTH
Sl. No
Mixes
Average compressive strength (N/mm2)
28days
56 days
1
GGBS0
32.33
32.55
2
GGBS1
31.33
33.22
3
GGBS2
30.55
35
4
GGBS3
29.66
36.55
5
GGBS4
28.55
35.66
6
GGBS5
27.77
33.66
7
GGBS6
25.67
32.78
3.5
3
2.5
2
1.5
1
0.5
Splitting Tensile Strength(N/ mm2)
3.5
3
2.5
2
1.5
1
0.5
Splitting Tensile Strength(N/ mm2)
0
0
Mixes
Mixes
Splitting tensile Strength (N/mm2)
Splitting tensile Strength (N/mm2)
Fig.2. Variation of splitting tensile strength for different mixes
Average compressive Strength (N/mm2)
Average compressive Strength (N/mm2)
c) Flexural Strength Test
Average 28th day compressive strength(N/ mm2)
Average 56th day compressive strength(N/ mm2)
Average 28th day compressive strength(N/ mm2)
Average 56th day compressive strength(N/ mm2)
0
0
Mixes
Mixes
40
35
30
25
20
15
10
5
40
35
30
25
20
15
10
5
Fig.1. Variation of compressive strength for different mix
b)Splitting Tensile Strength Test
TABLE 5 SPLITTING TENSILE STRENGTH OF CONCRETE
Sl. No
Mixes
Average Splitting Tensile Strength (N/mm2)
1
GGBS0
2.3
2
GGBS1
2.51
3
GGBS2
2.69
4
GGBS3
3.25
5
GGBS4
2.97
6
GGBS5
2.65
7
GGBS6
2.49
S Average Flexural Strength
Average flexural strength (N/mm2)
Average flexural strength (N/mm2)
l. No
Mixes
(N/mm2)
1
GGBS0
6
2
GGBS1
6.2
3
GGBS2
6.4
4
GGBS3
6.8
5
GGBS4
5
6
GGBS5
4.6
7
GGBS6
4
l. No
Mixes
(N/mm2)
1
GGBS0
6
2
GGBS1
6.2
3
GGBS2
6.4
4
GGBS3
6.8
5
GGBS4
5
6
GGBS5
4.6
7
GGBS6
4
TABLE 6 FLEXURAL STRENGTH OF CONCRETE
8
7
6
5
4
3
2
1
0
Average flexural strength( N/mm2)
8
7
6
5
4
3
2
1
0
Average flexural strength( N/mm2)
Mixes
Mixes
Fig.3. Variation of flexural strength for different mixes
On account of these mechanical properties of GGBS mixes, the mix obtained by cement replaced with 45% GGBS was taken as the optimum mix. A compressive strength of 56.55N/mm2 was obtained for this mix, which is almost in double of 25 N/mm2 being the design mix. Hence for further studies on polypropylene fibre reinforced GGBS mixes, specimens were cast with cement replaced with 45% GGBS and varying percentages of polypropylene fibre as 0, 0.1, 0.2, 0.3, 0.4 and 0.5%.
-
-
Experimental works for flexural & shear behavior
Experimental work of my thesis for the determination of effect of polypropylene fibre includes casting of twenty four beam specimens of 100mm breadth, 150mm depth and 1200mm length. Out of these, twelve specimens are used to study flexural behaviour and the remaining twelve specimens for the study of shear behaviour. The variables considered in this study are six different values of weight fraction of polypropylene fibres 0%, 0.1%, 0.2%, 0.3%,
0.4%, and 0.5%.
Flexural beams were provided with two numbers of 10mm diameter high yield strength deformed bars at bottom and two numbers of 8mm diameter bars at top. Two legged stirrups of 6mm diameter @ 90mm c/c have been used as shear reinforcement. Shear beams were provided with two numbers of 10mm diameter high yield strength deformed bars at bottom and two numbers of 8mm diameter bars at top. Two legged 6mm diameter stirrups were provided at the supports.
Fig.4. Reinforcement cage for flexural behaviour
Fig.5. Reinforcement cage for shear behaviour
TABLE 7 DETAILS OF SPECIMENS FOR TESTING FLEXURAL AND SHEAR BEHAVIOUR
Sl. No
Beam Designation
Polypropylene Fibre Weight (%)
No. of specimens (flexure+shear)
1
GGBSP0
0
2×2
2
GGBSP1
0.1
2×2
3
GGBSP2
0.2
2×2
4
GGBSP3
0.3
2×2
5
GGBSP4
0.4
2×2
6
GGBSP5
0.5
2×2
Total
12×2=24
C. Test setup
A two point flexural bending system is adopted for the tests. Specimens are tested in a loading frame of 2000 kN (200 t) capacity with an effective span of 1100 mm. Load cell of 200kN capacity with a least count of 1kN is used to measure the applied load.
Fig.6. Schematic diagram of loading
-
-
RESULTS AND DISCUSSION
TABLE 8 PROPERTIES OF FRESH CONCRETE
Sl. No
Mixes
Workability
Slump (mm)
Compacting factor
1
GGBSP0
30
0.85
2
GGBSP1
29
0.83
3
GGBSP2
28
0.81
4
GGBSP3
26
0.78
5
GGBSP4
25
0.75
6
GGBSP5
24
0.73
TABLE 9 TEST RESULTS FOR FLEXURAL BEAM SPECIMENS
Sl. No
Beam Designation
First Crack Load (kN)
Ultimate Load (kN)
Deflection at Ultimate Load
(mm)
1
GGBSP0
25
30
7.1
2
GGBSP1
39
44
7.4
3
GGBSP2
34
38
7.2
4
GGBSP3
28
33
6.9
5
GGBSP4
22
28
7
6
GGBSP5
18
26
6.8
TABLE 10 ENERGY ABSORPTION CAPACITY AND DUCTILITY INDEX
Sl. No
Beam Designation
Energy absorption (kNm)
Ductility index
1
GGBSP0
0.186
0.94
2
GGBSP1
0.276
1.32
3
GGBSP2
0.231
1.14
4
GGBSP3
0.193
1
5
GGBSP4
0.132
0.84
6
GGBSP5
0.105
0.78
0.3
0.25
0.2
0.15
0.1
Energy absorption capacity
0.3
0.25
0.2
0.15
0.1
Energy absorption capacity
0.05
0
0.05
0
Mixes
Mixes
Fig.7. Variation of energy absorption capacity for flexural beams
1.4
1.2
1
0.8
0.6
Ductility index
1.4
1.2
1
0.8
0.6
Ductility index
Mixes
Mixes
0.4
0.2
0
0.4
0.2
0
Ductility Index
Ductility Index
Fig.8. Variation of ductility Index for flexural beams
Beam Designation
First Crack Load (kN)
Ultimate Load (kN)
Deflection at Ultimate Load (mm)
GGBSP0
20
28
7.1
GGBSP1
29
39
7.4
GGBSP2
24
36
7.2
GGBSP3
19
32
6.9
GGBSP4
15
24
7
GGBSP5
11
22
6.8
Beam Designation
First Crack Load (kN)
Ultimate Load (kN)
Deflection at Ultimate Load (mm)
GGBSP0
20
28
7.1
GGBSP1
29
39
7.4
GGBSP2
24
36
7.2
GGBSP3
19
32
6.9
GGBSP4
15
24
7
GGBSP5
11
22
6.8
Fig.9. Comparison of load versus deflection curve for flexural beams TABLE 11 TEST RESULTS FOR SHEAR SPECIMENS
TABLE 12 ENERGY ABSORPTION CAPACITY FOR SHEAR SPECIMENS
Sl. No
Beam Designation
Energy absorption (kNm)
1
GGBSP0
0.102
2
GGBSP1
0.166
3
GGBSP2
0.145
4
GGBSP3
0.116
5
GGBSP4
0.087
6
GGBSP5
0.076
0.18
0.16
0.14
0.12
0.1
0.08
0.06
0.04
0.02
0
Energy absorption capacity
0.18
0.16
0.14
0.12
0.1
0.08
0.06
0.04
0.02
0
Energy absorption capacity
Mixes
Mixes
Fig.10. Variation of energy absorption capacity for shear beams
Fig.11. Comparison of load versus deflection for shear beams
Workability of concrete mix decreases with percentage addition of fibre. Compressive strength, flexural strength and splitting tensile strength increases by addition of up to 0.1% by weight of concrete. Percentage increase in 28th day compressive strength is 18% and 56th day compressive
strength is 12%. Percentage increase in splitting tensile strength of concrete is 55.5%. Percentage increase in flexural strength of concrete is 48.27%.
The addition of fibres up to 0.1% by weight of concrete improved the first crack load and ultimate load in case of flexural failure. The first crack load was found to have increased by about 56% at 0.1% weight fraction of fibres when compared to the specimens without fibres. The increase in ultimate load was found to be only 46.67%.
The toughness of reinforced concrete beams, increased as the weight fraction of polypropylene fibres increased up to 0.1%. Test results showed that the ductility increased significantly (16%) for beams with addition of polypropylene fibre 0.1% by weight of concrete. The addition of fibre also improved ultimate load by 39.29% and first crack load by 45% in case of shear failure of specimen up to 0.1% addition of polypropylene fibre. Crack width and number of cracks were less in case of fibre reinforced beam.
-
CONCLUSION
-
When fibre is added to concrete, the mix becomes stiff. So the workability is decreased with addition of fibre. The workability can be improved by adding super plasticizer to some extent.
-
The concrete mix starts clogging beyond the 0.1% addition of fibre. So the mechanical properties are decreased above 0.1% by weight of concrete.
-
The fibre distributes the strain more evenly in concrete and improves the tensile strength, thereby causing the increase in first crack load and ultimate load until clogging starts.
-
When fibres are added to concrete, crack propagation is arrested and this results in improving load carrying capacity and energy absorption capacity up to a certain limit. So the toughness and ductility is improved with the addition of percentage of polypropylene fibre up to the limit.
-
Load deflection behaviour curve shows that ductility of fibres increases up to the limit.
REFERENCES
-
Amit Rana(2013), Some studies on steel fibre reinforced concrete, International Journal of Emerging Technology and Advanced Engineering, 3, 120-127.
-
Aravindan S(2013), Experimental studies on fibre reinforced concrete from industrial waste, Journal of scientific research, 12, 1738-1744.
-
Chandra Sekhar Rao (2013), An investigation on confined fibre reinforced concrete beams under flexure, International Journal of Advanced Structures and Geotechnical Engineering, 2, 6-10.
-
Mukesh Shukla (2011), Behaviour of reinforced concrete beams with steel fibres under flexural loading, International Journal of Earth Sciences and Engineering, 4, 843-846.
-
Murali G (2012), Experimental investigation on fibre reinforced concrete using waste materials, International Journal of Engineering Research and Applications, 2, 278-283.
-
Pande A.M (2012), Experimental study on steel fibre reinforced concrete for M-40 grade, International Refereed journal of Engineering and science,1, 43-48.
-
Poornachand Pandit (2012), Experimental investigations on the flexural strength of reinforced concrete beams, International journal of earth sciences and engineering, 5, 1042-1045.
-
Rashid Hameed (2013), Flexural behaviour of reinforced fibrous concrete beams, International Journal of Engineering Research and Applications, 13, 19-28.
-
Sable K.S (2011), Performance of concrete beams under shear and torsion with fly ash and steel fibres, Elixir International Journal, 41, 6005-6008.
-
Sekar T (2004), Fibre reinforced concrete from industrial waste fibres, International Journal of Advanced Engineering Sciences and Technologies, 84, 287-290.
-
Shende A.M (2011), Comparative study on steel fibre reinforced cum control Concrete, International Journal of Advanced Engineering Sciences and Technologies, 6, 116-120.
-
Shirule Pravin Ashok (2012), Reuse of steel scrap from lathe machine as reinforced material to enhance properties of concrete, International Journal of Engineering Research and Applications, 2, 164-167.
-
Sravana P (2011), Some studies on flexural behaviour of glass fibre reinforced concrete members, International Journal of Structural and civil Engineering Research, 2, 110-115.