Development of Concrete Brick Using Recycled Plastic and Glass Waste

DOI : 10.17577/IJERTCONV11IS02026

Download Full-Text PDF Cite this Publication

Text Only Version

Development of Concrete Brick Using Recycled Plastic and Glass Waste

Akhil Mathai Varkey, Amaan Sajan, Aparna B Prasad

B.Tech students Dept. of civil engineering

Mangalam college of engineering Kottayam India

Athira Jacob Assistant professor

Dept. of civil engineering Mangalam college of engineering Kottayam India

Abstract The management of garbage is a critical issue in the modern world, particularly with regard to plastic and glass waste. Thousands of tonnes of plastic and glass are thrown in the trash every day, yet there aren't enough treatment and recycling options. Every day, a significant amount of plastic is thrown away or burned, contaminating the ecosystem and the atmosphere. Plastic trash buildup in the environment poses a threat to both plant and animal life. Recycling plastic and glass garbage after their useful lives are through while generating economic value and causing the least amount of environmental harm is the secret to their sustainable management in a circular economy. Bricks are a common building material used to make masonry structures like walls and pavement. Numerous research has been conducted on concrete that has been saturated with waste plastic and glass fiber, with positive outcomes and many benefits. Numerous testing have been carried out to manufacture eco bricks, including compression tests and water absorption tests.

Keywordsbricks; compression testing; water absorption testing

1.INTRODUCTION

One of the oldest and most common building materials is brick. Depending on their size, color, texture, origin, materials utilized, and forming process, the many varieties of bricks available on the market are employed. Bricks are an important component of industrial production processes in addition to being utilized in the construction of buildings. Plastic is a versatile, sturdy, and fairly priced material. These characteristics have led to the development of numerous products that are advantageous to society in terms of economic activity, employment, and level of living. Utilizing these waste materials is one way to address ecological and environmental problems. A such substance is glass, which is produced from raw materials like sand. Despite the fact that most glass debris is recycled in order to manufacture new glass products. Non- biodegradable and useful resource glass takes up valuable landfill space. In order to lessen the amount of glass waste

dumped in landfills, alternative recycling techniques must be investigated. The use of plastic and glass in such materials not only promotes their utilisation but also decreases the cost of making concrete and has other indirect advantages, including cheaper landfill costs, energy savings, and environmental protection from potential pollution consequences. Only a very small portion of it is recycled, most likely as a result of a lack of funding or a low level of interest in recycled plastic garbage. As a result, the majority of it is often burned or deposited in landfills. Such actions have a damaging impact on the environment at a time when the globe is concentrating its efforts on combating pollution and environmental challenges like global warming.

2.OBJECTIVE

To contrast the compressive strength and water absorption of standard concrete brick with bricks constructed using glass and polypropylene waste.

3.MATERIALS

  1. Cement: OPC grade 53 cement was used for the experimental work. According to IS standards, the cement was put through the following tests.

    Sl. no

    Tests

    Result

    1

    Fineness

    9%

    2

    Standard consistency

    32%

    3

    Initial setting time

    Less than 30 minutes

    4

    Final setting time

    10 hrs

    5

    Specific gravity

    3.06

    TABLE 1: Test on the cement

  2. Fine aggregate: In accordance with the IS standard, the aggregate was selected. Sizes of fine aggregate range up to 4.75mm.

TABLE 2: Test on fine aggregate

6.Glass wastes: Glass is amorphous (non-crystalline), which means it is more like a super-cooled liquid than a solid. Glass may be produced with exceptional uniformity in a range of shapes and sizes, from tiny filaments to large pieces.

Sl.no

Tests

Result

1

Specific gravity

2.65

2

Particle size distribution

Zone3, Fineness modulus 2.76, Uniformity

coefficient 2.5

3

Bulking of sand

Max bulking 35.2%, water content at max bulking 7%

4

Water absorption

1.25%

  1. Coarse aggregate: The size range up to 20mm was chosen for coarse aggregate.

    TABLE 3: Test on coarse aggregate

    Figure 2: Glass wastes

  2. MIX DESIGN

    Sl.no

    Tests

    Results

    1

    Specific gravity

    2.65

    2

    Grain size analysis

    Fineness modulus 5

    Uniformity coefficient 1.28

    3

    Water absorption

    1.55%

    M20 grade concrete was designed for the current investigation. The weight ratio of the mixture is 1:1.5:3, whereas the cement to water ratio is 0.5. It was suggested that the characteristics of brick be studied.

    TABLE 4: Mix proportion

    Proportion of plastic

    Proportion of glass waste

    Mix specification

    0%

    0%

    Conventional mix

    5%

    5%

    M1

    10%

    5%

    M2

    15%

    5%

    M3

    20%

    5%

    M4

    1. Water: Drinkable water is used for blending and conditioning of concrete.

    2. Plastic wastes: Due to its compactness and light weight, plastic has become the material of choice for reusable items in this period. In our study we used plastic.

      Figure 1: Plastic

      5.METHODOLOGY

      Common Portland cement OPC of 53 grade fine aggregate, coarse aggregate, water, and polypropylene plastic and glass wastes are employed in the study. Based on Indian standards,the analysis takes into consideration the obtained values as well as the cement, fine aggregate, and coarse aggregate qualities.M20 mix with mix proportion 1:1.5:3 is adopted for the study. For testing compressive strength and water absorption at 7, 14, and 28 days, nominal concrete was cast. Concrete bricks manufactured from recycled polypropylene plastic in varying percentages of 5%, 10%, 15%, and 20% and recycled glass in a constant percentage of 5% are cast and set for curing. Water absorption and compressive strength were calculated.

      Figure 3: Casting ,curing and strength testing of specimens

    3. RESULT AND DISCUSSION

    1. Compressive strength test

      Compressive testing demonstrates how the material will respond under compression. Using the compressive strength mehod, concrete bricks with various amounts of plastic and glass particles were tested for strength after 7, 14, and 28 days. Bricks with measurements of 400x150x200mm are cast for testing.

      TABLE 5: Compressive strength after 7,14, days

      Sl.no

      Mix specimen

      7 days N/mm2

      14 days N/mm2

      28 days N/mm2

      1

      M0

      13.17

      17.67

      20.16

      2

      M1

      13.5

      17.91

      20.5

      3

      M2

      13.75

      18.5

      20.75

      4

      M3

      14.33

      19

      21.16

      5

      M4

      13.58

      18.17

      20.47

      7.CONCLUSION

      In this study, concrete brick development employing glass and plastic trash that has been recycled is discussed. This study also tries to appropriately utilize waste materials since plastic and glass are waste products that are bought from the local scrap market. Several studies, including as compressive strength tests and water absorption tests, are used to look into the characteristics of the plastic and glass bricks. It has been discovered that 15% is the ideal replacement rate for coarse aggregate when replacing it with plastic and glass waste; anything higher than 15% reduces the compressive strength of the brick.

    2. Water absorption test

An absorption test on the material is done to find out how much moisture a brick will take in under harsh conditions. By comparing the weights of dry and wet bricks, it is possible to calculate the quantity of water absorption. A brick should not absorb more water than 20% of its dry weight after being submerged in water for 24 hours.

Sl.no

Brick(%)

Dry weight(kg)

Wet Weight(kg)

Water absorbed(%)

1

0

22.94

23.740

3.4

2

5

22.53

23.410

3.9

3

10

20.17

20.950

3.8

4

15

19.5

20.1

3.07

5

20

18.63

19.40

4.13

TABLE 8: Water absorption

8.REFERENCE

  1. Erfan Najaf, Hassan Abbasi, Using recycled concrete powder, waste glass powder and plastic powder to improve the mechanical properties of compacted concrete: cement elimination approach (2022) https://doi.org/10.1155/2022/9481466

  2. Ilham I. Mohammed, Nazim Abdul Nariman, Kaywan Othman, Sarhad Ali, Peshwaz Mohammed, Sirwan Samad , Utilization of waste plastic and waste glass together as fine and coarse aggregate in concrete (2020) http://dx.doi.org/10.23918/eajse.v6i2p1

  3. Aneke Frank Ikechukwu, Celumusa Shabangu , Strength and durability performance of masonry bricks produced with crushed glass and melted PET plastics (2021) https://doi.org/10.1016/j.cscm.2021.e00542

  4. Gowtham R , S Manikanda Prabhu , M Gowtham , R Ramasubramani , A review on utilization of waste glass in construction field (2021) https://www.researchgate.net/publication/350865506

  5. Pooja Lamba, Dilraj Preet Kaur, Seema Raj , Jyoti Sorout , Recycling/reuse of plastic waste as construction material for sustainable development : a review (2021) https://doi.org/10.1007/s11356-021-16980-y

  6. Merna Amir Kamal, Rania Rushdy Moussa , Marianne Nabil Guirguis , Recycled Plastic as an Aggregate in Concrete (2021) http://dx.doi.org/10.13189/cea.2021.090502