- Open Access
- Total Downloads : 296
- Authors : Habibi Samir, Ziadi, Abdelkader, Megeni Abdelkader
- Paper ID : IJERTV2IS80174
- Volume & Issue : Volume 02, Issue 08 (August 2013)
- Published (First Online): 24-08-2013
- ISSN (Online) : 2278-0181
- Publisher Name : IJERT
- License: This work is licensed under a Creative Commons Attribution 4.0 International License
Assessment Of Mechanical Properties Of Biphased Steel By The Small Punch Test And Design Of Experiment Methods
Habibi Samir
Université de Sidi Bel Abbes, Laboratoire de mécanique des structures et des solides, Algérie, and Faculté de Technology, Département de Génie mécanique, Algérie
ZIADI ABDELKADER
Centre universitaire dAin Témouchent, Laboratoire des structures intelligentes, Algérie.
MEGENI ABDELKADER
Université de Sidi Bel Abbes, Laboratoire de mécanique des structures et des solides, Algérie, and Faculté de Technology, Département de Génie mécanique, Algérie
Abstract
The characterization of biphased steel structure led us to exploit the experimentat results of a study which consists in the determination of local properties of different steels invastigated [1].The present work is a comparative study between the emperical relation (CENCWA 15627(part A) )[2] and the two relations examined by S.D.Norris and J.D.Parker [3], concerning the estimtion of the ratio of mechanical strength over maximum local with respect to the geometric properties of the indentation apparatus and the thickness of the specimen. We propose a mathemtical model of type 23 factorial plan to express the ratio using the characteristic variables of the apparatus.
Key words: small punch test (SPT), mechanical resistance over maximum load, design of experiment, statistical tools.
-
Introduction
During the small punch test, the material is subjected to a uni-axial stress, plastically deformed, cracked up to rupture. Small punch test (SPT), conducted in five DP steels show the ductile behavior of steels from plots of the excerced force on the specimen with respect to displacement. Design of experiment is a method to ameliorate the quality. The success of the original planning is its possibility to interpret experimental results with a minimum effort in experimentation. The minimization of the number of experiment reduces time and cost. The work performed to find the best cerelation between mechanical resistance and maximum load are conditioned by dimensional standards of indentation set up. This limits the application and exploitation of the computational methods for different experimentatal set up. The objective of this study is the verification of S.D.Norris and J.D.Parkers method, [3] for the determination of the mechanical ratio with respect to geometrical parameters of the small punch test appratus. The specimen used are made of dual phasd steel which has a good deal between resistance/drawing. This emanate from the microstructure made of hard phase (martensite or bainite) dispersed in ductile ferritic matrix. The consolidation capability induced by the deformation of these steels is considerable. A statistical analysis of the small punch test has been made using design of experiment with a general linear model.
-
Description of the experimental device
Figure 1. Small punch testing device [2]
-
Experimental resullts
Five steels with carbon content (<20%) have been used in the experimental study conducted by [1]. The main mechanical properties of thes steels are grouped in table 1.
Table 1. Mechanical properties obtained by SPT [1]
Specimen
Pmax (N)
m (Mpa)
Py (N)
ys (Mpa)
dmax (mm)
2
1941,75
700
382,75
460
1,325
3
1955,25
825
401,5
460
1,38
4
1979,75
870
476,25
632
1,365
5
1445,75
990
496
622
0,84
6
1689,25
1101
590,75
874
0,835
DP 5
DP 6
DP 5
DP 6
0,725
0,700
0,675
m /Pmax , mm-2
m /Pmax , mm-2
0,650
0,625
0,600
0,575
0,550
DP 2
DP 2
0,525
DP 3
DP 3
DP 4
DP 4
0,500
0,475
The small punch test (SPT) is a method considered in practice to be non-destructive because of the reduced size of the specimen (10*10mm2), and 0.5mm in thickness. The SPT can measure directly the mechanical properties of the materials [4]. The test consists in integrating the entire contour of the specimen which is maintourned between two dies (3,4), then after to deform the specimen up to rupture using the punch(2) with spherical lead of 2.5mm in diametr. A extensiometer (5) is used to determing the stress-strain plot through the lower die (3) (with 4mm in diameter)of the indentation apparatus as shown in figure 1:
1,0 1,1 1,2 1,3 1,4 1,5 1,6 1,7
DIsplacement at fracture dF , mm
Figure 2. Characteristic curve of indentation tests of the DP steels
The values of the displacement at rupture have been extracted from figure 2. The statistical serie recording the ratio (mechanical resistance over max load ) of the five DP steels investigated in [1] are given in table 2.
Table 2. Maximum mechanical ratio (
dF [mm]
1.57
1.58
1.60
1.07
1.09
m/Pmax
[mm-2]0.36049
0.42194
0.43945
0.68476
0.65177
-
-
Method of determination of the mechanical ratio
-
Normative method (cen cwa 15627)
Replacing the geometrical characteristic by their values (R= = 2mm, p = 1.25mm, t = 0.5mm).
In the emperical equation [2]
= 3.33.Ksp. . .t (3.1)
we obtain : = 1.891.Ksp (mm2) (3.1.1) This confirm the demonstration of Yang Z and Wang Z.W,
[5] using Newtons polynomial development taken from Chakrabartys theory[6].= 1.72476. – 0.05638. 2 0.17688. 3 (3.2)
Thus = 1.891 mm2 if =1.6 mm [7].
if Ksp =1 (CEN CWA 15627, Hyde and Sun., 2009) then = 1.891
giving = 0.52882 (3.3)
-
S.D.Norris and J.D.Parkers method
3.2.1 Nomenclature and equations Equations (3.4) and (3.5) rad been examined by S.D.Norris and J.D.Parker[3].
= (3.4)
= (3.5)
with Cl=A-(d+2t) (3.6)
: Ultimate strength (Mpa)
= Maximum load (N)
Cl : Clearance of the dies
t : thickness of specimen (0.5mm)
D : sphere diameter (indentor) (2.5mm) A : Lower die diameter (4mm)
: Displacement at rupture (mm)
Considering equations (3.4) and (3.6) we obtain :
= (3.7)
We obtain a constant ratio, by using the values of dimensions of the experimental set up we obtain :
= 0.3384 (3.8)
From formula (3.5), we express the ratio ( ) with respect to the displacement at rupture (dF) we obtain :
=
(3.9) Thus we obtain using the second formula the values of the ratio shown in table 3.
Table 3. Maximum mechanical ratio of DP steels
Désignation Steel
dF
[mm][mm-2] 2
1.57
0.50673
3
1.58
0.50396
4
1.60
0.49850
5>
1.07
0.69884
6
1.09
0.68850
-
-
Proposed model by design of experiment
The study of the small punch test apparatus can be schematized as follows :
We are interested in a quantity Y called response which dependent on a certain number of variables X1, X2, X3 called factors.
The mathematical modeling consists in measuring the response Y for many valuesof variables Xi by maintaining the fixed the other two variables. We iterate this method for each of the variables.
The design of experiment method proposes a factorial experimentation [8] i.e all the factors vary simultaneously. The handling of the results is made by multiple linear regression and variance analyses.
4.1. Choice of the factors and experimental domain
The factors are supposed to be the parameters that influence the response which characterizes the behavior of the phenomenon under investigation.
It is important to be able to attribute two levels for each factor, a low and a high level. The low level is coded by (-1) and the high level is coded by (+1). Table 4 shows the factors of the model
Table 4. Designation of the factors
N
Désignation
Abreviation
1
Constant
Cst
2
Thickness
t
3
Radius of lower die
R
4
Radius of indentor (sphere)
p
5
Thickness * Radius of lower die
t*R
6
Thickness * Radius of indentor
t*p
7
Radius of lower die * Radius of indentor
R*p
8
Radius of lower die * Radius of indentor * Thickness
R*p*t
The plan for which each of the three factors has only two levels is called 23 plan. Thus the corresponding table is :
Table 5. Choice of the level of the factors
Factors
Units
Type
level
t
mm
Quantitatif
0.20 – 0.50
R
mm
Quantitatif
0.75 – 2.00
p
mm
Quantitatif
0.50 – 1.25
-
Experimental matrix
The matrix of experiment is a table which indicater the number of experiment to carry out, their order and the way to vary the factors.
Table 6. matrix of experiment
-
Graphical analysis of the results
Yates method has been used for the caculation of the effects. The originality of this method is that can allow directley to find the general formula e of the average effects [8].
4.3.1 Analysis of the effect of parameters on the mechanical ratio A graphical illustration of the results allows easy interpretation of the obtained information.
Figure 3 : shows the effect of each parameter on the mecanical ratio
Effect of the three factors studied
Thickness, mm
0,15 0,20 0,25 0,30 0,35 0,40 0,45 0,50 0,55
2,8
Experience
t
R
p
1
0.2
0.75
0.5
3.25
2
0.5
0.75
0.5
1.30
3
0.2
2
0.5
3.96
4
0.5
2
0.5
1.58
5
0.2
0.75
1.25
1.08
6
0.5
0.75
1.25
0.43
7
0.2
2
1.25
1.32
8
0.5
2
1.25
0.53
Experience
t
R
p
1
0.2
0.75
0.5
3.25
2
0.5
0.75
0.5
1.30
3
0.2
2
0.5
3.96
4
0.5
2
0.5
1.58
5
0.2
0.75
1.25
1.08
6
0.5
0.75
1.25
0.43
7
0.2
2
1.25
1.32
8
0.5
2
1.25
0.53
2,6
2,4
2,2
2,0
Ratio
Ratio
1,8
1,6
1,4
1,2
1,0
Factor 1: Thikness
Factor 2: Spherical punch
Factor 3: Lower die
This table is composed of high (+1) and low (-1) levels. The response Y expresses the ratio of ultimate stress to ultimate load we use an experimental plan of 23 using a factorial matrix with Yates algorithm [8]. The results are given in table :
Table 7. Presentation of experimental plan 23(annex 1)
4.2.1 Estimation of coefficients of the model The coefficient of the model are obtained using modde 6.0. It can be observed that a1,a2 and a3 are well the average effects of factors X1,X2 and X3. The coefficient a0 is the theorical response at the center of the domain of variation of the factors.
The model is written as:
Y = a0 + a1.X1 + a2.X2 + a3.X3 + a12. X1. X2 + a23. X2. X3 + a13. X1. X3 + a123. X1. X2. X3 (4.1)
Or Y = 1.682 – 0.721X1 + 0.164X2 – 0.842X3 – 0.070 X1 X2 – 0.082 X2 X3 + 0.360 X1 X3 + 0.036X1 X2X3 (4.2)
The variables X1, X2, X3 designate the variables t, R, respectively. The model can be expressed as:
= 1.682 – 0.721.t + 0.164.R – 0.842.p – 0.070.t.R –
0.082.R.p + 0.360.t.p + 0.036.t.R.p (4.3)
or = fct (t, R, r, t.R, R.p, t.p, t.R.p)
0,8
0,6
0,50 0,75 1,00 1,25 1,50 1,75 2,00 2,25
Radius of the lower die, mm
0,4 0,6 0,8 1,0 1,2 1,4
Radius of the spherical punch, mm
Figure 3. Effects of the factors on mechanicals ratio
The plots of the average effects of the parameters give immediate observation of in important factors.
The spherical indenter has the highest effect on the maximum variation of load indentation, then the effect of the lower die which has low influence on the reponse.
-
Analyse of interaction effects
Figure 4. Graphical representation of interaction between the three factors (annex 1).
In each of these graphs, the existence of interaction is detected when the lines are not parallel. In the case under investigation the interactions are relatively low. A low interaction between the indenter and the lower die can be observed : more the size of the spherical indenter is important, more the variation of the thickness allows to increase the load of indentation.
-
Paretos diagram It is possible to decompose the variation of the response from the contribution of factor in a model.
Figure 5. Paretos diagram of the three factor and their contributions
Paretos diagram, [9] is a complement of the plot of the average effects. The contribution and the analysis of paretos diagram for obtaining a aximum mechanical ratio put into evidence the predominance of the role of the factor size of the spherical indenter (p) which appears first with the longest histogram. From the histogram we can notice that the factor indenter (p) and the thickness (t) explain the 70% of the variation of the response. The contribution of the third factor the diameter of lower die is very lowand represents only 07.41%.
-
Variance analysis
The variance analysis (ANOVA) allows to compare the variance of cumulated values of the model with that of residuals. This analysis is a statistical test Gaudoin [10] (Fisher-Snedecor).
Table 8. ANOVA
-
Test of the significtion of coefficients
The coefficients of the factors and those of interactions necessitate test of signification. The statistical calculations which allow if the effects are significant, to calculate the confidence intervals or to validate the model linearity make intervene the residuals i.e the difference
between the experimental value and the value predicted by the model, and an estimator of variance of residuals.
For the estimation and the significance the effects of coefficients a students test is used [8].
Table. 9. Residuals
The results and the values of the statistical test with the coefficients are grouped in table10 :
Table. 10. Ponderation of the effects
Variable
Effect
Result
Constant
a0 = 1.682
Significant
t
a1 =- 0.721
Significant
R
a2 = 0.164
Significant
p
a3= – 0.842
Significant
t.R
a12=- 0.070
Non Significant
R.p
a23=- 0.082
Non Significant
t.p
a13 = 0.360
Significant
X1. X2. X3
a123= 0.036
Non Significant
This table shows that the variables t, R, p and the interaction (t.p) are significant.
It is clear that the average of the response given by a0 is the most dominant, which explains that the effect of all the factors is important. It can be observed that the action of indentor (p) is the most significant before the thickness of the specimen (t) and before the diameter of the lower die. Only the interaction shown by (t.p) is significant. The interactions showns by (t.R) and (R.p) wich are not significant this means that the effect is not, with the given risk, significantly different from 0. That is the variables associated to a12, and a23 have no effect on the response.
The result of the test recommand to take a model of the form:
=1.682 – 0.721.t + 0.164.R – 0.842.p + 0.360.t.p (4.4)
-
Response surface
These responses are presented the two different ways. The first in space with a curved surface, the second is the projection of the surface on a plan called iso-response, [9]:
Figure 6. Contour of response of the variation of mechanical ratio (annex 2).
The first curve reprented by the blue zone which is the inferior part of the graph corresponds to a lighter influence of the parameters as shown by the small variation of response which less than 0.95 mm-2. Even with greater size of the indentor up to a radius of 1.25 mm, one note that this is due to the mon significant effect of the lower die
less than 0.8 mm.
The analysis of the rest of the zones (yellow, orange and red). The whole are under the form of a triangle with a pick representing a critical point to which all points converge. This means that the behavior of the material changes to another state. This can be a plastic deformation or rupture.
One note that this zone corresponds to an important variation of the response with respect to the preceding cases. We reach a maximum ratio of 2.75 mm-2 which comes from the interaction of two parameters, the increase of the matrix radius up to 2 mm and the decrease of the radius of the punch at least 0.55mm.
We also note that this zone correspond to an important variation reaching a maximum ratio of 2.49 mm-2 due to the interaction of two parameters increase of matrix radius up to 1.6 mm and the decrease of the specimen thichness at least 0.2 mm.
The analysis of the third curve shows that the simultaneous decrease of two parameters shows that the variation of the response is inversely proportional simultaneous decrease of the thickness and the punch radius can give a maximum increase of the response that reaches 3.27 mm-2 for 0.25 mm thickness and 0.6 mm punch radius.
It is clear for an increase of the thickness and the punch radius the variation of the response is alternative and instable. It has been noticed that for a constant thickness, the increase of punch radius lowers the response. For a constant punch radius the increase of the thickness increases the response.
The simultaneous increase of these two parameters results into a compensation.
-
-
Results and discussion
Table. 11. Gives a summary of the obtained results
(annex 2)
– The variance and standard deviation: The couple variance and standard deviation [8] are estimated as (0.017, 0.13) for the first case and (0.011, 0.11) for the third case. Both values of the couples are too close for the two cases. The average deviation of value of the ratio is small and the variance low. Thus the scores are concentrated around the calculated average.
-The coefficient of variation : First case X=0.52816,S= 0.13 and CV1= 25.6% and third case X= 0.56440, S= 0.11 and CV3=18.50%
The values of the series of the ratios of the third case have less deviation from their center than that of the first case. They are less dispersed and are homogeneous. The degree of dispersion of the two distribution stoys closer with a 5% tolerance.
The two relative dispersion converge to the same center average value of the first case 0.52816 and 0.56440 of the third case with a tolerance of 3.6%.
-
The average of the ratios : From the statisticl analysis of the first study (Cardenas and al., 2009) first case, the average is 0.52816 which is conform to the normative method (4th case) with an average value of 0.52882. The calculation of the ratio by Norris and Parkers method using the second formula gives a value of 0.56440 closer to the normative value and that of the first case with only a tolerance of 6% .
-
The experimental design : The experimental design gives a new expression by giving a ratio estimted of 0.54700 with 3% deviation from that of the normative method.
Through the experimental design we observe :
-
The increase of the thickness of the indentation specimen decreases.
-
The increase of the size of the sphere lowers the response.
-
The interaction of the increase of the size of the sphere with the decrease of the thickness of the specimen increase the response.
-
The simultaneous increase of these two parameters results in a compensation.
The ratio of the ultimate stress over the maximum load is aqual to 0.33840 for the second case using Norris and Parkers first formula which shows a value far from the average calculated values with an important deviation of 36%.
-
-
Conclusion
The statistical tools have allowed to analyse the expression of the variation of the mechanical properties with respect to the dimensional parameters of small punch test devices. We have shown that S.D.Norris and J.D.Parkers second formula is applied to the obtained results (1).
The characterization of the five DP steels by (SPT) gives results conform to the normative method .
This can be explain by the fact that the ratio is a function of the displaceent at rupture.
It has been verified that S.D.Norris and J.D.Parkers first formula which is an empirical formula expressing the ratio wich respect to the dimensions of small punch test devices appratus and the thickness of the specimen gives a constant result far from the normative method.
The first formula does not take into consideration the mechanical properties of the steels but only the parameters R, r and t.
References
-
E. Cardenas, C. Rodriguez, F.J. Belzunce y C. Betegon 2009, estudio de las propiedades mecanicas de aceros de doble fase mediante el ensayo miniatura de punzonado, Anales de Mecanica de la Fractura 26, Vol. 1.
-
CEN CWA 15627 2006, Workshop Agreement: Small punch test method for metallic materials (Part A), (European committee for standardization).
-
S. D. Norris and J. D. Parker 1996, deformation processes during disc bend loading, Matrials Science and Technology, 12, 8, 163-170.
-
Lucas G.E. et al., 2002, recent progress in small specimen test technology, J. Nucl, Mater., 307-311, 1600-1008.
-
Yang, Z. and Wang, Z.-W 2003, relationship between strain and central deflection in small punch creep specimens, Int. J. Pressure Vessels Piping, 80, 397-404.
-
Chakrabarty, J 1970, a theory of stretch forming over hemispherical punch heads, Int. J. Mech. Sci., 12, 315-325.
-
Autillo, J 2006, Contreras M.A. , Betegon C., Rodrigez C., Belzunce F.J., utilizacion del ensayo miniatura de punzonamiento en la caracterizacion mecanica de aceros, Anales de Mecanica de la fractura, 23, 77-83.
-
Goupy, j. et Creighton, L 2006, Introduction aux plans dexpériences, DUNOD.
-
Pillet, M., 2001, Les plans dexpérience par la méthode Taguchi, les éditions dorganisation.
-
Gaudoin, O 2009, principes et méthodes statistiques, ensimag- 2ème Année, INP Grenoble.
-
T.H.Hyde, W.Sun 2009, high-sensitivity, small specimen creep test, Journal Strain Analysis Vol.44.
Annex 1
Table 7. Presentation of experimental plan 23
Experience |
Average |
X1 |
X2 |
X3 |
X1. X2 |
X2. X3 |
X1. X3 |
X1. X2. X3 |
Yexp |
1 |
+1 |
-1 |
-1 |
-1 |
+1 |
+1 |
+1 |
-1 |
3.25 |
2 |
+1 |
+1 |
-1 |
-1 |
-1 |
+1 |
-1 |
+1 |
1.30 |
3 |
+1 |
-1 |
+1 |
-1 |
-1 |
-1 |
+1 |
+1 |
3.96 |
4 |
+1 |
+1 |
+1 |
-1 |
+1 |
-1 |
-1 |
-1 |
1.58 |
5 |
+1 |
-1 |
-1 |
+1 |
+1 |
-1 |
-1 |
+1 |
1.08 |
6 |
+1 |
+1 |
-1 |
+1 |
-1 |
-1 |
+1 |
-1 |
0.43 |
7 |
+1 |
-1 |
+1 |
+1 |
-1 |
+1 |
-1 |
-1 |
1.32 |
8 |
+1 |
+1 |
+1 |
+1 |
+1 |
+1 |
+1 |
+1 |
0.53 |
Divisor |
8 |
8 |
8 |
8 |
|||||
Effects |
a0=1.68 |
a1=- 0.72 |
a2=0.16 |
a3=- 0.84 |
a12 =-0.070 |
a23 =-0.082 |
a13= 0.360 |
a123 = 0.036 |
4.3.2 Analyse of interaction effects
Fig. 4. Graphical representation of interaction between the three factors
Figure 6. Contour of response of the variation of mechanical ratio.
Table. 11. Gives a summary of the obtained results
Ratio [mm-2] |
Standard |
Coefficient of variation |
Absolut average |
|||
Emperical Formula |
deviation |
CV |
deviation |
|||
Géométric Charactéristic of SPT device |
Méchanical Properties of Material |
|||||
EMA |
||||||
S |
||||||
1/ Statistics of study [1] |
0.52816 |
Résultats expérimentaux (Traction/SPT) |
0.13 |
25.6 % |
0.12 |
|
2/ Norris and Parker formula (3.4) |
0.33840 |
|||||
3/ Norris and Parker Formula (3.5) |
0.56440 |
0.11 |
18.5 % |
0.10 |
||
4/ Normative Méthod |
0.52882 |
3.33. Ksp.R-0.2.r 1.2.t |
||||
5/ Design of experiment 23 |
0.54700 |
1.682 – 0.721.t + 0.164.R – 0.842.p – 0.070.t.R – 0.082.R.p + 0.360.t.p Or KSP (1.682 – 0.721.t + 0.164.R – 0.842.p + 0.360.t.p) |