An Experimental Study on Fibre Reinforced Concrete Using Polypropylene Fibre and Partial Replacement of Coarse Aggregate by Weld Slag Material

DOI : 10.17577/IJERTCONV6IS07015

Download Full-Text PDF Cite this Publication

Text Only Version

An Experimental Study on Fibre Reinforced Concrete Using Polypropylene Fibre and Partial Replacement of Coarse Aggregate by Weld Slag Material

Nivedhan R1*, Nivedhitha V1*, Rifakkathullah A1*, Sowmiya S1*,

1. UG students, Department of Civil Engineering,

M.A.M College of Engineering and Technology

Mr . P. Gopalsamy2

2. Assistant professor, Department of civil engineering,

      1. College of Engineering and Technology

        Abstract – Normal or conventional concrete uses more of the raw material like sand, gravels, fly ash etc. its usage has been increased to an enormous amount where there are likely chances of meeting with the demand of such construction materials. It may also lead to increase the cost of the materials drastically. To overcome such situations, alternate building materials were emerging now-a-days. This study has been made as an attempt in improving the technological ailment by using recycled materials for construction. Weld Slag and Fibres, the abundantly available materials were selected for partially replacement in concrete. Weld Slag being a residual content is used in concrete with various proportions as a partial replacement of coarse aggregate in the proportion of 10%, 20% and 30% by weight. Polypropylene fibre being used for the post cracking purpose in concrete is used here for increasing the mechanical properties of the concrete along with the addition of Weld Slag. The fibre is added at the proportion of 0.2% of total volume of the concrete. This experimental investigation is carried out to evaluate the ability to increase the mechanical properties of the concrete by using Weld Slag and polypropylene fibre and to determine the optimum dosage of those ingredients.

        1. INTRODUCTION

          The present day, world is facing the construction of very challenging and difficult civil engineering structures. Concrete, being the most important and widely used material, is called upon to possess very high strength and sufficient workability properties.

          The advancement of concrete technology can reduce the consumption of natural resources and energy sources and less the burden of pollutants on environment. The construction materials which have been using till now may create a huge demand in the future due to lack of availability. It is effective that the waste comes from weld industries can be used in concrete as a replacement for normal construction materials such as aggregate. Presently large amount of waste weld materials are generated in the industries. Concrete is strong in compression as they aggregate efficiently carries the compression load. However, it is weak in tension as the

          cement holding the aggregate in place can crack, allowing the structure to fail. Reinforced concrete adds steel reinforcing bars, steel fibres, polymer fibres, glass fibres or plastic fibres to carry tensile loads. Fibre reinforced concrete (FRC) is concrete containing fibrous material which increases its structural integrity. While concrete brittleness to a large extent can be compensated with steel reinforcement on structural scale in fibre reinforced concrete resulting in improved structural durability, safety as well as improved performance in infrastructure sustainability. Polypropylene fibres are widely employed in the reinforcement of concrete as they present some advantages including, high durability of the fibre reinforced concrete, they have a greater effect on reducing the shrinkage of concrete and they reduce of the spalling effect in high strength concrete subjected to elevated temperature. The effect of polypropylene fibres is more pronounced in the elastic modulus due to shrinkage cracking reduction and on the fracture behavior of the fibre reinforced concrete due to the bridge effect of the crack lips.

          OBJECTIVES OF THE WORK

          • To study the utilization of waste materials as partial replacement of aggregates in concrete.

          To investigate the mechanical properties of the concrete using weld slag and polypropylene fibre.

          SCOPE OF THE WORK

          Weld slag as a partial replacement for coarse aggregate with 10%,20% and 30%

          Polypropylene fibre as adding material with 0.2%.

        2. LITERATURE REVIEW

          A comparison has been made plain cement concrete and the fibre concrete containing weld slag in various proportions by weight. The workability of fresh weld fibre reinforced concrete is restricted to less weld contents. The compressive strength of weld fibre

          reinforced concrete is found to be maximum for (28 days strength) weld slag fibre added concrete. The addition of weld slag in concrete has increase the performance of beam in flexural by 40% when compared with PCC. The replacement of coarse aggregate by weld slag is found to be very effective. Concrete gets early strength and hence shuttering can be removed early thereby reducing the secondary overhead cost.

          POLYPROPYLENE FIBRE

          Fibers are plying an increasing role as the reinforcing medium of choice for concrete construction. Specifications of polypropylene fibre are given in the table.

        3. MATERIAL USED CEMENT

          Lots of factor impacts on the strength of concrete, but strength of cement is the most important and direct factor. Portland Pozzolana cement of 43 grade conforming to IS 8112-1989 is used. Specific gravity of cement is 3.09.

          FINE AGGREGATE

          Natural river sand is used as fine aggregate. The properties of sand are determined by conducting tests as per IS: 2386(part-1). The results are shown in the table. The results obtained from sieve analysis are furnished

          Table 1 Physical properties of fine aggregate

          SI. No

          Properties

          Values

          1

          Specific gravity

          2.66

          2

          Water absorption

          1.15%

          COARSE AGGREGATE

          Properties of the coarse aggregate affect the final strength of the hardened concrete and its resistance to disintegration, weathering, and other destructive effects. 20mm size of coarse aggregate is used. The properties of coarse aggregate are shown in table.

          Table 2 Physical properties of coarse aggregate

          SI. No

          Properties

          Values

          1

          Specific gravity

          2.67

          2

          Water absorption

          0.85%

          WELD SLAG

          Replacing weld slag for coarse concrete as 10%,20% and 30% in the concrete. Specific gravity of weld slag is 2.83

          Fig 1 Weld slag

          Fig 2 Polypropylene fibre

          Table 3 Specification of PF

          Type

          Austenitic

          Length (l)

          38mm

          Diameter (d)

          0.4-0.6cm

        4. METHODOLOGY Proposed Mix Design:

          The aim of the experiment is to investigate the behavior of the polypropylene fibre and weld slag when partially replaced by coarse aggregate in cubes, cylinders and prisms. The Mix adopted is M30 (1: 2.13: 3.67), designed as per IS 10262:2010.

          Mixes

          Water

          Cement

          Fine

          Aggregate

          Coarse

          Aggregat

          Polypropylene

          Fibre

          Weld

          Slag

          M1

          150

          340

          725

          1249

          M2

          150

          340

          725

          1124.1

          0.0136

          124.9

          M3

          150

          340

          725

          999.2

          0.0136

          249.8

          M4

          150

          340

          725

          874.3

          0.0136

          374.7

          Table 4 Mix Proportions (1m3 of concrete)

        5. EXPERIMENTAL WORKS

To test the concrete for compression (150mm x 150mm x150mm), split tensile strength (300 mm length with 150 mm diameter) and flexural strength (500mm x 100mm x100mm) were cast respectively. Specimen is obtained for 7 and 28 days.

Fig 3 Test of concrete

GRAPH RESULT

Fig 5.2 comparison of compressive strength of concrete at 7 days

Fig 5.2 comparison of compressive strength of concrete at 28 days

V1 RESULT AND DISCUSSION 1.COMPRESSIVE STRENGTH ON CONCRETE CUBE

Table 5.1 Compressive strength of cube for 7 days

S.No

Age of test

Percentage of

weld slag

Compressive strength

2

N/mm

1

7 days

0

16.31

2

7 days

10

16.93

3

7 days

20

18.15

4

7 days

30

19.08

Table 5.2 Compressive strength of cube for 28 days

SI.no

Age of test

Percentag e of Weld slag

Flexural strength

2

N/mm

1

28 days

0

3.33

2

28 days

10

4.01

3

28 days

20

4.31

4

28 days

30

4.7

VII CONCLUSION

Experimental tests are conducted and Mechanical properties of concrete such as compressive strength, splitting tensile strength and flexural strength are determined for conventional concrete and weld slag replaced concrete cast at various mix proportions. The strength parameters of conventional concrete and weld slag fibre reinforced concrete are compared. The test results of hardened concrete were shown that there is a considerable increase in Compressive strength, Flexural strength and Tensile strength. The weld slag fibre reinforced concrete test was conducted for 10%, 20% and 30%. By increasing the percentage of weld slag, all the strengths also increased. Hence 0.2% will be an optimum percentage of the fibre reinforced concrete for high strength concrete and hence weld slag fibre reinforced concrete is used in construction

Fig5.3 comparison of compressive strength of concrete for 28 days

  1. SPLIT TENSILE STRENGTH ON CONCRETE CYLINDER

    Table 5.3 Splitting tensile strength of cylinder

    GRAPH RESULT

  2. FLEXURAL STRENGTH ON CONCRETE PRISM Table 5.4 Flexural strength of prism

s.no

Age of test

Percentage of wed slag

Compressive strength N/mm2

1

28 days

0

37.43

2

28 days

10

37.57

3

28 days

20

38.02

4

28 days

30

38.75

GRAPH RESULT

Fig 5.6 Comparison of flexural strength of concrete at 28 days

VII CONCLUSION

Experimental tests are conducted and Mechanical properties of concrete such as compressive strength, splitting tensile strength and flexural strength are determined for conventional concrete and weld slag replaced concrete cast at various mix proportions. The strength parameters of conventional concrete and weld slag fibre reinforced concrete are compared. The test results of hardened concrete were shown that there is a considerable increase in Compressive strength, Flexural strength and Tensile strength. The weld slag fibre reinforced concrete test was conducted for 10%, 20% and 30%. By increasing the percentage of weld slag, all the strengths also increased. Hence 0.2% will be an optimum percentage of the fibre reinforced concrete for high strength concrete and hence weld slag fibre reinforced concrete is used in construction

s.no

Age of test

Percentage of weld slag

Split tensile strength

N/mm 2

1

28 days

0

2.72

2

28 days

1

0

3.29

3

28 days

2

0

3

. 5

0

4

28 days

3

0

3.73

REFERENCES

  1. 1. Shetty M.S.,2002, Concrete

    Technology,S.Chand and Company Ltd. Ramnagar, New Delhi.

  2. IS: 10262-1982 Concrete Mix Design.

  3. IS: 383 Sieve Analysis.

  4. IS: 456-2000 Table 5, Water Cement ratio.

  5. 5. Meriem Senani, Noureddine Ferhoune,

  6. Abdelhamid Guettala (2016), Substitution of the natural sand by crystallized slag of blast furnace in the composition of concrete Alexandria University of Alexandria Engineering Journal.

  7. R.K. Mishra, R.K. Tipathi, Vikas Dubey (2016), Early age shrinkage pattern of concrete on replacement of fine aggregate with industrial by-product Journal of radiation research and applied sciences.

  8. Manoj Kumar Dash, Sanjaya Kumar Patro, Ashoke Kumar Rath (2016), Sustainable use of industrial- waste as partial replacement of fine aggregate preparation of concrete Gulf Organisation for Research and Development of International Journal of Sustainable Built Environment.

  9. Dinesh W. Gawatre, Poorva Haldkar, Shraddha Nanaware, Ashwini Salunke, Meherunnisa Shaikh, Anita Patil (2016), Study on addition of lathe scrap to improve the mechanical properties of concrete International Journal of Innovative Research in

    Sciences, Engineering and Technology ISSN 2319- 8753,Vol 5, Issue 5.

  10. Maggi Madrid, Aimar Orbe, Eduardo Roji, Jesus Cuadrado (2017), The effects of by-products incorporated in low-strength concrete for concrete masonry units Constructions and Building Materials 153(2017) 117-128. 10. P.M. Dhureen Karthik, S. Krishna Prasanth, M. Annapoorna, R.

  11. Shanmugasundaram (2016), An experimental study on mechanical properties on fibre reinforced concrete using polypropylene and marble powder International Journal of Science Technology and Engineering (IJSTE), Vol 3, Issue 6.

  12. Jingjun Li, Jiangang Niu, Chaojun Wan, Xiaoqin Liu, Zhiyi Jin (2017),

  13. Comparison of flexural property between high performance polypropylene fibre reinforced lightweight aggregate concrete and steel fibre reinforced light weight aggregate concrete, Constructions and Building Materials 157(2017) 729-736.

  14. Kutalmus Recep Akca, Ozgur Cakr, Mertin Ipek(2017), Properties of polypropylene fibre reinforced concrete using recycled aggregates, Constructions and Building Materials 98(2015) 620- 630.

  15. Hector Cifuentes, Fidel Garcia, Orlando Maeso, Fermando Medina (2013), Influence of the properties of polypropylene fibres on the fracture behavior of low-

    , normal- and high-strength FRC, Constructions and Building Materials 45(2013)130-137.

  16. 15. Salahaldein Alsaey, Muhsen Salem (2016), Influnce of polypropylene fibre on strength of concrete, American Journal of Engineering Research(AJER) , ISSN 2320-0936, Vol 5,Issue 7.