Comparative Study of Bearing Materials and Failure of Plain Bearings
S. B. Chikalthankar1, V. M. Nandedkar2, P. V. Jawale3
1,3 Department of Mechanical Engineering, Government Engineering College, Aurangabad, India.
2 Department of Production Engineering, SGGS Institute of Engineering and Technology, Nanded,India
Abstract The first part of this paper highlights the general requirements of bearing materials and bearing material properties. The different causes of failure of plain bearings along with remedies to avoid them are discussed. The research work related to failure of bearings is presented.
Keywords Hydrodynamic Lubrication, Score Resistance, Deformability, Fatigue, Wear
-
INTRODUCTION
An actual bearing is much more than some bearing material wrapped around a shaft or held against a moving bearing. A bearing is a machine element that must be properly designed. Practical design considerations of bearings include deformation of the bearing shell, length to diameter ratio, misalignment, heat transfer and heat dissipation capacity, clearances, allowable pressures and various mechanical and thermal construction details. The bearing material is only one component of an overall integrated design. A bearing may still fail even when employing the best bearing material if the design of the unit is faulty [1].
-
THE PLAIN-BEARING ENVIRONMENT
To determine the choice of a bearing material it is useful to recognize four main types of bearing applications:
-
Reciprocating engine bearings operating with hydrodynamic lubrication, a dynamic load being applied to the bearing surface through the oil film. The best- known examples are the big-end and main bearings of the automotive engine. This bearing application is of particular importance, not only because of the sheer volume of internal combustion engines now produced, but because the high oil-film pressures generated over the bearing surface have provided an important impetus in bearing materials development.
-
Rotating plant bearings operating with hydrodynamic lubrication, the load applied to the bearing surface through the oil film being steady. Examples are turbine journal bearings, rolling-mill bearings, marine stern tubes, tilting-pad thrust bearings.
-
Lubricated bearing applications operating under conditions that do not create full hydrodynamic lubrication. This category covers the common copper-based alloys, used-oil- or grease-lubricated in general engineering applications, as well as graphited bronze, wick-lubricated whitemetal, and the
important classes of oil-impregnated porous bronze bearing and prelubricated plastic or plastic-lined bearings.
-
Non-lubricated bearing applications, i.e. bearings operating dry or in non-lubricating media. For such applications the most commonly used bearing materials are those based on the polymer polytetrafluoroethylene (or ptfe) [2].
-
-
GENERAL REQUIREMENTS OF BEARING MATERIALS
-
Score resistance
-
Mutual Solid Solubility
-
Compressive strength
-
Fatigue strength
-
Deformability
-
Corrosion resistance
-
Structure
Bearing materials are selected on the basis of applications and which properties are of prime importance in that application.
-
Score Resistance:- The anti-weld or anti-seizure characteristic of a bearing material is referred as score resistance. White metals are used where score resistance is of prime importance. Improved score resistance is obtained at the expense of loss of hardness or strength. Table I shows the relative order of common bearing metals with regard to score resistant tendencies.
TABLE I.
Bearing Materials
Order of Score Resistance
Order of Inherent hardness or strength
Application
Aluminium Alloys
3
1
For heavily loaded moderate speed bearings
Copper Leads
2
2
For heavily loaded high speed bearings
White Metal alloys
1
3
Low to moderately loaded, low to high speed bearings where dirt and deflection are
present
-
Mutual Solid Solubility: Early work by Ernst and Merchant showed that the mutual solid solubility between metal pairs was a very significant parameter in predicting friction and wear. Table 2 lists scoring resistance of elements against stee
TABLE II.
Good
Fair
Poor
Very Poor
Germanium
Carbon
Magnesium
Beryllium
Silver
Copper
Aluminium
Silicon
Cadmium
Selenium
Copper
Calcium
Indium
Cadmium
Zinc
Titanium
Tin
Tellurium
Barium
Chromium
Antimony
Tungsten
Iron
Thallium
Cobalt
Lead
Nickel
-
Compressive Strength: – It is the ability of the material to carry imposed load without extrusion or disintegration.
Sr.
No.
Bearing Material
Order of Fatigue Strength
Order of
deformab ility
1
Bronzes
1
7
2
Copper Lead with tin or silver
2
6
3
Thin-Babbit overlays
3
5
4
Aluminium alloys
4
4
5
Copper-Lead
5
3
6
Cadmium alloys
6
2
7
Lead and
Tin based babbits
7
1
-
Fatigue Strength: Engine bearings such as main and connecting rod bearings of crankshafts must carry high alternating loads. Automotive connecting rod bearings sometimes reach pressures of 27.6 MPa based on projected area. Actual peak pressure in the oil film may exceed the average pressures by a factor of 5 or 6 and hence magnitude of alternating stresses is severely high. Bronze has high fatigue strength but has low deformability. Table 3 shows fatigue strength and deformability of typical bearing materials
-
Deformability: The ability of a bearing material to yield to deformation while operating without causing
failure is highly important. When loads are applied to the structure the bearings and journals deflect often leading to edge contact. Tin base babbitt is able to wipe out locally relieve any high spots or areas of metallic contact and then reform its contour to re- establish fluid film contact.
-
Corrosion resistance: The corrosive aspects of Bearing materials are important especially in engine bearings when high automobile sump temperatures caused an epidemic of oil oxidation and deterioration and the frmation of acid. This acid proceed to attack vigorously and effectively on new bearing materials resulting in disastrous results [1]. Table III List the Corrosion Resistance of Bearing materials:
TABLE III.
Non-corrodible
Intermediate
Corrodible
Aluminium alloys
Bronzes
(High Lead)
Cadmium Alloys
Tin-base Babbitt
Copper-Lead
Lead base Babbitt
Alkali
hardened lead
Cadmium
Indium alloys
Silver
Bronzes (low lead)
-
-
-
MATERIALS FOR THE CRANKSHAFT BEARINGS OF THE
HIGH SPEED INTERNAL COMBUSTION ENGINE
The selection of bearing material in High Speed Internal Combustion Engine depends upon:
h) The Engine Bearing Environment an oil film, thickness of the film, pressure generated in the film and temperature attained in the film.
-
Maximum Oil Pressure of the order of 140-210 N/mm2
-
Minimum oil film thickness in the region of 5 m
-
Maximum oil film temperature 100-170oC
-
Cavitation
-
WhitemetaI Engine Bearing Alloys:
Tin- and lead-based whitemetals, Le. Tin antimonycopper or lead-antimony-tin alloys, have excellent compatibility, and being soft (20-30 HV) have good conformability and ability to embed dirt. Their corrosionresistance is in general very good. Unfortunately, their resistance to fatigue is, by the standards of present-day engines, poor. In UK a tin-based alloy (89 Sn, 7·5 Sb, 3·5 Cu) is used for high speed engines. In USA lead-based whitemetal to SAE15 (83 Pb, 15 Sb, 1 Sn, 1 As) is still used fairly widely in automobile engines.
-
Copper-Lead and Lead-Bronze Engine Bearing Alloys
High-lead, copper-lead alloys, with lead contents in the range 25-50%, were introduced in the US in the 1930's, and are still used in that country under the broad classification of intermediate' bearing alloys [2].
-
-
ENGINE BEARING FAILURES
-
Bearing failures due to metal-to-metal contact
Mixed lubrication is one of the main causes of engine bearing failures. Metal-to-metal contact may appear in the following forms of bearing wear:
-
Accelerated wear: is when the bearing is not overheated and only a shiny appearance of the bearing surface is observed.
-
Wiping or heavy wear: this appears in the form of overheating and partial melting of the overlay (the left part of the Fig.1).
-
Severe wear or Hot Short: it results in torn surfaces, severe overheating, melted overlay and lining material (right part of the Fig.1).
Causes of mixed lubrication and the methods of solving the problem are presented in the table below:
Bearing failures due to metal-to-metal contact
Cause
Solution
Insufficient oil supply (oil starvation)
Check oil supply system (e.g. clean clogged oil
passages ,insufficient clearance, etc)
Breaking the oil film (due to oil contamination or
bearing material fatigue)
Change bearing material (tri-
metal instead of bi-metal) or solve overloading problem
Misalignment (e.g. out-of-shape grinding, distorted
connecting rod)
Correct deficient machining, fix/replace distorted parts
Poor journal surface finish
Verify proper grinding/polishing
procedures
Foreign particles embedded in the bearing surface
Determine origin of particles, improve cleaning
procedures prior to assembly.
Clean parts with hot soapy water. Do not clean with solvents
Low viscosity oil (diluted with fuel or coolant)
Identify/address source of oil dilution, use higher
viscosity oil
Grinding chatter marks (waviness) and lobing
TABLE IV.
-
-
Engine bearing failures due to fatigue
Bearing material fatigue is the second cause of bearing failure. Fatigue of an aluminum lining. The fatigue cracks form on the surface and propagate inside the lining reaching the steel back. The cracks then progress along the bond line between the lining and the steel. Pieces of the lining flake out from the steel back resulting in oil contamination and eventual bearing
failure. Fatigue of aluminum alloys may also cause extrusion of the lining material past the length of the bearing edges.
Fatigue of a tri-metal overlay. Spider web-like cracks are seen on the surface (Fig.4). Fatigue limit of an overlay is determined by the strength of the material and the thickness of the overlay. The thinner the overlay, the higher its fatigue strength. Overlay fatigue itself does not cause the bearing to fail. However, running the bearing with fatigued overlay may cause partial flaking of the overlay, lowering the oil film thickness and eventual seizure of the exposed intermediate layer.
Fatigue of a copper based intermediate layer. Fatigue of a copper based lining (Fig.4) starts from a fatigue of the overlay. The overlay flakes out from the copper lining resulting in an interruption of the oil film, breaking the hydrodynamic lubrication regime. The load localizes at the contact area causing formation of small cracks on the lining surface. The cracks then propagate throughout the lining thickness, meeting the steel back surface and continuing to advance along the steel-copper boundary. As a result, parts of the intermediate layer detach from the steel surface.
Engine bearing failures due to fatigue
Cause
Solution
Wrong selection of engine bearing material
Change to a bearing material with higher load capacity (e.g.tri-metal instead of bi-
metal)
Fuel detonation /
advanced ignition
Retard ignition or use a fuel
with higher octane number
Running engine at high torque and low RPM for a
long time (climbing)
Change to bearing material with higher load capacity (e.g. tri-
metal instead of bi-metal)
Poor conforming of the bearing back with
the housing surface
Oil starvation causing localization of load at particular bearing areas
Check oil supply system for clogged oil passages, check clearances, component geometry, oil pressure +
volume
Geometry misalignments causing localization of
bearing loading
Fix/replace distorted parts or use more conformable material
(bi-metal instead of tri-metal)
Corrosive action of
contaminated oil enhancing Fatigue
Eliminate/diminish oil dilution
or use oil with corrosion inhibiting additives
-
Check the bearing crush height
-
Properly re-size the housing
The table below shows factors that cause fatigue and methods of preventing bearing failures due to fatigue.
-
-
Geometric irregularities
Fig. 5 and 6 show examples of the effect of geometric irregularities. Both problems are seen in the picture: local wear with shiny appearance and the overlay fatigue in form of spider web like cracks on the areas of metal-to-metal contact.
Distorted (bent or twisted connecting rod) is one of the causes of localized loading of engine bearings (Fig.5). Overloading of an internal combustion engine due to detonation or running under hightorque at low rotation speed may cause distortion of the connecting rods. The distortion results in non-parallel orientation of the bearing and journal surfaces. The non-parallelism causes localized excessive wear
of the bearing surface due to metal-to-metal contact (boundary or mixed lubrication) occurring near the bearing edge. Localized metal-to-metal contact may also cause fatigue cracking of the bearing material in the locations of the contact.
Imperfect journal geometry is another cause of localized loading of engine bearings (Fig. 6). Use of a worn stone in grinding a crankshaft results in obtaining an imperfect (out-of- shape) journal surface: taper shape, hour glass shape or barrel shape. The parts of the journal surface having higher diameter (central part of the barrel shape journal, edge parts of hour glass shape journal) come to metal-to metal contact (boundary lubrication) with the bearing surface. The metal-to-metal contact causes excessive wear. Fatigue cracking of the bearing materials may occur in the contact areas.
-
Cavitation erosion of the overlay
Cavitation erosion is another type of engine bearing failure differing from both fatigue and metal-to-metal contact. Cavitation is a phenomenon related to hydrodynamics. Cavitation occurs when the load applied to the bearing fluctuates at high frequency (high RPM). The oil pressure instantly falls causing formation of bubbles (cavities) due to fast evaporation. When the pressure rises the cavitation
bubbles collapse at high velocity. Such collapse results in impact pressure, which can erode the bearing material (Fig.7). Soft lead based overlays of tri-metal bearings are prone to the cavitation erosion. Therefore replacement of tri-metal bearings with babbitt overlay with bi-metal material or with high strength tri-metal bearings (e.g. GP) will prevent the failures due to cavitation [3].
Fig.7 Cavitation erosion of soft lead based overlay
-
-
CONCLUSION:
The failure of bearing materials not only depends on the bearing materials, their proper selection it is greatly affected by the working conditions of the bearings. The common causes of engine bearing failure and their remedies are discussed in this study. A judicious attempt has to be made while selecting the bearing materials and compromising between the properties of the bearings while selecting the material for a particular bearing application.
REFERENCES
-
Dudely D. Fuller Theory and Practice of Lubrication for Engineers, 2nd Edition April 1984 p. 619-628
-
G.C. Pratt. Materials for Plain Bearings, International Metallurgical Reviews 1973, Vol 18
-
Dr. Dmitri Kolpelivioch Engine Bearings Failures and How to avoid them, King Engine Bearings Inc.
-
King Engine Bearings Inc. Engine Bearing Materials
-
Dr. Dmitri Kolpelivioch Engine Bearings and How they work, King Engine Bearings Inc.