- Open Access
- Total Downloads : 1350
- Authors : Abhijitsinh Parmar, Dhaval M Patel
- Paper ID : IJERTV2IS121218
- Volume & Issue : Volume 02, Issue 12 (December 2013)
- Published (First Online): 28-12-2013
- ISSN (Online) : 2278-0181
- Publisher Name : IJERT
- License: This work is licensed under a Creative Commons Attribution 4.0 International License
Experimental Study on High Performance Concrete by Using Alccofine and Fly Ash – Hard Concrete Properties
Abhijitsinh Parmar*, Dhaval M Patel**
*Assistant Professor, SVBIT, ** ME WRM, LDCE
Abstract
India is developing country and now days skyscrapers and other heavy structures are constructing and for that high performance concrete requires. The search for alternative binders, or cement replacement materials, has been carried out for decades. Research has been conducted on the use of fly ash, volcanic ash, volcanic pumice, pulverized-fuel ash, blast slag and silica fume as cement replacement material. Fly ash and others are pozzolanic materials because of their reaction with lime liberated during the hydration of cement. The main aim of this study is to get the economical and eco friendly High Strength Concrete(HSC). The fresh concrete test carried out for finding properties of this concrete at Harden stage.
-
Introduction
A pozzolan is siliceous or siliceous and aluminous material which, in itself, possesses little or no cementitious value but which will, in finely divided form and in the presence of water,
react chemically with calcium hydroxide at ordinary temperature to form compounds possessing cementitious properties (ASTM C618).[1]
Concrete is mostly used artificial material all over the world and has played main role in development of all countries. For higher and higher requirements in last past few years many research has been done on concrete t make it more durable and higher strength. In 1970s compressive strength more than 40 N/mm2 known as high- strength concrete. Later 60-100 N/mm2 compressive strength classified as High-strength concrete
High performance concrete is used for concrete mixture which possess high workability, high strength, high modulus of elasticity, high density, high dimensional stability, low permeability and resistant to chemical attack.
CEMENT (%)
FLY ASH (%)
ALCCOFINE (%)
M1
70
26
4
M2
70
24
6
M3
70
22
8
M4
70
20
10
M5
70
18
12
Table 1 Mix Proportion of Cement, Fly ash and Alccofine
As per M60 Mix design in this research the Alccofine and fine fly ash partially replaced with cement. Replacement of cement with fly ash and Alccofine of 5 proportions are shown in table -1
-
Pozzolonic Reactions
This is a chemical mechanism. Reactive silica (SiO2) of pozzolan reacts with the calcium hydroxide (CH), which is liberated during process of hydration and produces calcium silicate hydrate (C-S-H). Due to pozzolonic reaction the larger size of crystal of Ca (OH)2 converts to crystal of C-S-H, which is dense and leading to reduction of pore size.
Portland cement Reaction : C3S + H = C-S-H + CH Pozzolonic Reaction : S + CH + H = C-S-H
-
-
Objectives
The main objective of this project is to study the properties of fresh and hardened high performance concrete. It consists of following point
-
To achieve desire strength of (M60).
-
To find out optimum dosage of alccofine.
-
To reduce the cost of concrete by finding out the optimum dosage of fly ash.
-
To find out compressive strength , flexural strength and split tensile strength of concrete.
-
To perform the non destructive test on concrete specimen.
-
-
Materials
Physical and Chemical Properties of Fly ash and Alccofine shown in table 2, table 3, table 4 and table 5 respectively
Sr. No
Character
Results
1
Lime reactivity , N/mm2
8 min
2
Retention On 25 Micron Sieve
>0.5
3
Drying Shrinkage, percentage
0.06
4
Soundness by Autoclave expansion, percent
0.05
5
Compressive Strength, as percent of strength of corresponding plain cement mortar cubes
80
Table – 2 Physical Composition of Fly Ash
Sr No
Type of test
Test Method
Result obtained
1
CaO%
IS-1727
0.50
2
SiO2%
IS-1727
67.60
3
Al2O3%
IS-1727
11.30
4
MgO%
IS-1727
0.10
5
SO3%
IS-1727
0.06
6
NaO2%
IS-4032
0.035
7
K2O%
IS-4032
0.005
8
Total Chloride%
IS-12423
0.008
9
Loss on Ignition%
IS-1727
2.60
10
Fe2O3%
IS-4031
1.15
11
TiO2%
IS-4031
Nil
12
P2O3%
IS-4031
0.0002
Table -3 Chemical Composition of Fly Ash
Fineness (cm2/gm)
Specific Gravity
Bulk Density (Kg/m3)
Particle Size Distribution
D10
D50
D90
12000
3.11
700-900
1.5
5
9
Table-4 Physical Composition of Alccofine
Cao
So3
Sio2
Al2O3
Fe2O3
MgO
Cl
61-
64%
2-
2.4%
21-
23%
5-
5.6%
3.8-
4.4%
0.8-
1.4%
0.03-
0.05%
Table-5 Chemical Composition of Alccofine
-
Experimental Program
To find out harden properties of concrete following test were carried out.
-
Ultrasonic pulse velocity test.
-
Rebound hammer test.
-
Compressive strength of concrete cubes.
-
Split tensile strength of concrete cylinder.
-
Flexural strength of concrete beam.
Proportions of 5 groups and quantity of materials per m3 are shown in table 6.
M60
M1
M2
M3
M4
M5
CEMENT
(kg)
414.4
414.4
414.4
414.4
414.4
FLY ASH(kg)
46.176
42.624
39.072
35.52
p>31.968 ALCCOFINE
(kg)
7.104
10.656
14.208
17.76
21.312
WATER
(kg)
258.5
258.5
258.5
258.5
258.5
C.A 1(kg)
755.5
755.5
755.5
755.5
755.5
C.A 2(kg)
752
752
752
752
752
Sand(kg)
173
173
173
173
173
Water(kg)
414.4
414.4
414.4
414.4
414.4
Table 6 Mix Proportions
-
Ultrasonic pulse velocity
Figure 1 UPV test
Direct Ultrasonic Pulse Velocity test were carried out as shown in figure 1. For each proportion upv test carried out in 3 samples and average result shown in table -7
-
Rebound Hammer Test
Figure 2 Rebound Hammer test
Rebound hammer test was carried out as shown in figure 2. Results of Rebound hammer test are shown in table – 8
-
Compressive Strength
Figure 3 Compression Test
The compressive strength was studied on different ages of concrete, with different proportion of Alccofine and Fly ash in the concrete mix. This is the long term strength study, thus we have selected different age of concrete such as 7 Days, 28 Days and 56 Days. The cube mould of 150mm x 150mm x 150mm size is taken as per IS: 516-1959 specification.
-
Split Tensile Strength
Figure 4 Split Tensile Strength
The split tensile strength was made as per the IS: 5816- 1999 specification, on the Grade M60 with different Alccofine and Fly ash percentage. For this study the concrete cylinders of diameter 150mm and height 300mm were prepared. Total 3 Nos. of cylinders were cast for each Alccofine proportion in the concrete mix,
i.e. total 45 nos. of cylinders prepared for this test. Cylinders were cured for 28 Days time age.
-
Flexural Strength
Figure 5 Flexural Test
The beam flexural strength was made as per the IS: 516-1959 specification, Concrete Grade M60 with different Alccofine and fly ash percentage. For this study the concrete beams of size 150mm x 150mm x 700mm were prepared. Beams were cured for 28 Days time age. The beams were tested on the Universal Testing Machine (UTM). The beams were placed normal to the casting and symmetrical two point system was adopted for the flexural tensile strength test.
-
-
-
Test Results
Proportion
M1
M2
M3
M4
M5
7 Days
4.52
4.63
4.60
4.53
4.66
28 Days
4.66
4.64
4.63
4.50
4.56
56 Days
4.64
4.59
4.62
4.59
4.67
Table 7 UPV Test Results
Proportions
M1
M2
M3
M4
M5
7 Days
32.39
34.57
37.01
39.25
40.47
28 Days
57.18
52.73
61.05
52.91
59.79
56 Days
60.17
62.34
60.71
61.6
61.93
Table 8 Rebound Hammer Test Results(N/mm2)
Mix proportion
M1
M2
M3
M4
M5
7 Days
37.51
37.62
42.33
42.73
46.52
28Days
59.31
56.14
66.64
56.71
63.74
56Days
66.09
70.51
67.2
64.51
68.15
Table 9 Compression Test Results(N/mm2)
Mix proportion
M1
M2
M3
M4
M5
28 Days
3.73
4.01
4.63
4.19
4.3
56 Days
4.89
4.22
5.08
4.41
4.75
Table 10 Split Tensile Test Results(MPa)
Mix proportion
M1
M2
M3
M4
M5
28 Days
6.03
4.91
5.57
6.58
6.37
Table 11 Flexural Strength
-
Conclusion
-
Non-Destructive Test
By doing Non destructive test like Ultrasonic Pulse Velocity & Rebound Hammer we get excellent quality of concrete as per IS 1311(part- 1 & 2).
-
Compressive Strength
In all mix proportions strength gain up to 7 days is excellent, between 7 to 28 days strength gain is comparatively less, but between 28 to 56 days strength gain is high because of fly ash, in M3 proportion get acceptable strength at 28 days as per Table-7, clause 6.2.1 of IS 456-2000.
It concluded that initial compressive strength achieved by using Fly-Ash (22%) and Alccofine (8%) is 42.33 Mpa and 66.64 Mpa at 7 and 28 days respectively, but after 28 days strength gain is comparatively less than other.
-
Split Tensile Strength
After testing the split tensile strength of cylinder we concluded that cylinders are not getting tensile strength up to desired limits of 5.42 Mpa but in most of the cases the failure was in aggregates and not in transition zone of paste so it may be covered by using some different gradation or by using high strength aggregates.
Maximum split tensile strength of cylinder was achieved 5.08 Mpa in M3 mix (fly ash- 22% and alccofine-8%).
-
Flexural Strength
After testing flexural strength test of beam concluded that maximum flexural strength of 6.58 Mpa in M4 mix (fly ash-20% and alccofine-10%).
-
-
References
-
Mehta, P.K. (1987). Natural pozzolans : Supplementry cementing materials in concrete. CANMET Special Publication 86: 1-33.
-
K.aniraj S.R. and Havangi V.J.(Aug 1999).
Geotechnical Characteristics of Fly ash soil mixture Geotechnical Engineering Journal, 30 pp 129147
-
IS 456 -2000, Plain and Reinforced Concrete code for Practice.
-
IS 10262- 2009, Recommended Guidelines for Concrete Mix Design.