Influence of Microfine GGBS on Concrete of Grade M35 & M40 Made with Pozzolana Cement

DOI : 10.17577/IJERTV5IS100252

Download Full-Text PDF Cite this Publication

Text Only Version

Influence of Microfine GGBS on Concrete of Grade M35 & M40 Made with Pozzolana Cement

Balram Sharma ¹

¹M.Tech Student , Department of Structural Engineering,

Kautilya Institute of Technology, Engineering and School of management, Sitapura, Jaipur, India

Abstract In this study development of concrete by making an efficient concrete mix design blending with mineral admixtures on micro fine GGBS for higher grade concrete has been undertaken. Development of efficient concrete mix design plays an important & vital role in producing eco-economical concrete. This study represents the effect of presence of mineral admixture micro fine GGBS.GGBS partially replaced & added in cement concrete for evaluating the workability and strength of concrete along with flexural & split tensile strength. This study has been done by varying (5% to 25%) GGBS on partial replacement & addition in cement by weight of Portland pozzolana cement. About twenty-four trial mix, control mix and other variation mix were developed for M35 & M40 grade of concrete. Compressive strength 7 days and 28 days using cube (150mm x 150mm x 150mm) specimen, flexural strength for 28 days using beam (700mm x 150mm x 150mm) and splitting tensile strength for 28 days using cylinder (300mm length x 150mm diameter) were evaluated for this study by casting these in institute lab. All these concrete specimens were cured for 7 days and 28 days in deep water tank on normal 27+20C degree atmospheric temperature.

Keywords High grade concrete, compressive strength, mix design, GGBS, workability, flexural strength and splitting tensile strength.

  1. INTRODUCTION

    Concrete is building material made of coarse aggregate, fine aggregate making pure matrix required water and cement. At present many type of concrete technologies, its application improves construction work in durability, strength and thermal resistance condition.

    A. Supplementary Cementitious Materials / Mineral admixture

    Mix design of concrete play an important role for the concrete and mix design of concrete give standard design for better performance and desired strength ability. At present the concrete development is based on the use of industrial wastage such on supplementary cementitious material. Industrial wastage has pozzolanic as well as cementitious properties. There have very fine grained-particles; having Cementitious Materials improve the properties of concrete mix. This type of Cementitious Materials called, Supplementary Cementitious Materials. Mineral admixtures such on GGBS improve the concrete strength, low cost of preparation, thermal resisting and improved durability. A good concrete mix requires workability, strength and

    S. D. Thanvi ²

    ²Associate Professor

    Kautilya Institute of Technology & Engineering,

    Sitapura, Jaipur, India

    durability. Silica fume is also been used as mineral admixture, it increases the strength and durability. Pozzolanic material fly ash and GGBS have very fine particles. Silica fume have 100 times small particles compare to Fly ash/cement, it give high surface-to-volume ratios compare to fly ash. GGBS also is a good mineral admixture. It is used to partially replace Portland cement. Silica fume is similar to fly ash/GGBS as mineral admixture, but has a particle size 100 times smaller. All mineral admixture surface- volume ratios give higher value and good pozzolanic action.

  2. EXPERIMENTAL PROGRAM

    1. Introduction

      Concrete is a mixture of cement, sand, coarse aggregate and water. Evaluate the performance of concrete containing supplementary cementations materials such micro fine GGBS. Cement replaced with Mineral admixtures can recover the strength and durability of concrete. The challenge for civil engineering community to improve the properties of concrete and concrete has eco-friendly condition.

      In present concrete required economic & good blending material property. So, some industrial wastes use as blending material to improve property of concrete.

    2. Materials

      Concrete is a composite material of coarse aggregate, fine aggregate, water and cement. A good concrete mix requires workability, strength and durability.

    3. Coarse Aggregate

      • Coarse aggregate Particle sizes more than 4.75mm and in this experimental work uses 10mm and 20 mm aggregates.

        Concrete mixture makes up majority of Fine and coarse aggregates. In concrete mix uses aggregates like natural gravel, Sand and crushed stone. The concrete a true composite material when the coarse aggregate are presence greatly and necessary cement material composite it proper type. That type material makes a brittle and high strength composite.

        TABLE I. PROPERTIES OF COARSE AGGREGATE 10MM &20MM

        Tests

        Coarse Aggregate

        10mm

        20mm

        Density (SSD)

        1478 kg/m3

        1560 kg/m3

        Sp. Gravity (SSD)

        2.66

        2.66

        Water Absorption

        0.43%

        0.44%

    4. Fine Aggregate

      Fine aggregate (sand) particle size less than 4.75mm sieve and Sand shall be fresh hard, hard-wearing, angular, sharp, and free from mica, silts, and alkalis, organic and vegetable matters. It should not contain more than 5% of clay or silt. Sand should be perfectly drying before measured. IS code specification classifying the fine aggregate Zone-1 to Zone- 4grade.Fine aggregate passing percentage various sieves and there are mainly four zones and they all have different passing percentage.

      TABLE II. PROPERTIES OF FINE AGGREGATE

      Tests

      Coarse Aggregate

      Density (SSD)

      1675 kg/m3

      Sp. Gravity (SSD)

      2.64

      Water Absorption

      1.20 %

    5. Cement

      Cement is binding material in the cement concrete. It is used for various engineering works where strength and durability are of Prime importance. Cement property depend upon quantity of water in cement concrete. Potable water is required to make a good concrete. PPC has fly ash in cement it react calcium hydroxide and produces calcium silicate hydrate. Calcium silicate hydrate gives strength and durability and makes eco-friendly.

      Chemical reaction of OPC & PPC In OPC

      Chemical Analysis

      Mass%

      CaO

      36-40

      Al2O3

      5-5.6

      Fe2O3

      3.8-4.4

      SO3

      2-2.4

      MgO

      6.5-8

      SiO2

      30-34

      Chemical Analysis

      Mass%

      CaO

      36-40

      Al2O3

      5-5.6

      Fe2O3

      3.8-4.4

      SO3

      2-2.4

      MgO

      6.5-8

      SiO2

      30-34

      2[2CaO.SiO ] + 4[H O] = [3(CaO)2(SiO )3(H O)] +

    6. Admixture

      Admixture is components in concrete other than coarse aggregate, fine aggregate Portland cement and water. It leads main role make concrete good composite material. Admixture use primary hardening an workability or deliver extra properties for concrete mix.

      Type of admixture

      • mineral admixture

      • chemical admixture

        1. Mineral admixture (Micro fine Ground granulated blast slag

          Well-ordered granulation procedure with high reactivity found Micro fine GGBS. It has high glass content. The processing with other select constituents results in under controlled partial size distribution (PSD).The calculated blain value based on PSD is about 9000cm2/gm and is actually ultrafine. Micro fine GGBS delivers condensed water demand for assumed workability, even up to 70% replacement and addition near as per condition of concrete performance. Micro fine GGBS can also be used as a great range water reducer to recover compressive strength or as a super workability add to improve flow. Micro fine GGBS is pozzolanic materials that can be used to produce highly hard- wearing concrete composites.

          TABLE IV. PHYSICAL PROPERTIES OF MICRO FINE GGBS

          Physical Analysis

          Range

          Bulk Density

          700-900 kg/m3

          Surface Area(finesse)

          9000cm2/gm

          Particle Shape

          Irregular

          Specific gravity

          2.9

          TABLE V. CHEMICAL PROPERTIES OF MICRO FINE GGBS

          2 2 2 2

          Ca(OH)2

          (OPC) (Water) (C S H) (Free Lime)

          In PPC

          2[2CaO.SiO2] + 4[H2O] = [3(CaO)2(SiO2)3(H2O)] +

          Ca(OH)2

          (OPC) (Water) (C S H) (Free Lime)

          3[Ca(OH)2] + 2[SiO2] = [3(CaO)2(SiO2)3(H2O)]

          Properties

          Range%

          CaO

          50-60

          SiO2

          36-40

          Al2O3

          6-8

          MgO

          0.1-3

          SO3

          1-3

          Na2O

          0-1

          Fe2O3

          4-5

          Specific Gravity

          3.00

          Properties

          Range%

          CaO

          50-60

          SiO2

          36-40

          Al2O3

          6-8

          MgO

          0.1-3

          SO3

          1-3

          Na2O

          0-1

          Fe2O3

          4-5

          Specific Gravity

          3.00

          (Free lime) (Silica from Fly ash) (C S H) TABLE III. PROPERTIES OF CEMENT PPC 43 MPA

        2. Chemical Admixture

        Chemical admixtures are material in the form of powder or fluids which are added to the concrete to reduce the water in plain concrete mixes. Water reducing super plasticizer used in this experimental work. Plasticizers increase the workability of plastic or "fresh" concrete, permitting it is sited more simply, with fewer consolidating strength. Plasticizers can be castoff to decrease the water contented of a concrete while improving workability and are called water-reducers due to this usage. Naptha based water reducing superplasticizer as per IS9103:1999used.The superplasticizer which is used for the experimental performance is Shaliplast SP-431. Properties of Chemical Admixture

        Type of admixture

        Super plasticizer chloride free & IS: 9103

        SP. GRAVITY@27ºC

        1.20 +/- 0.04

        DRY MATERIAL %

        41- 45 %

        CHLORIDE %

        NIL

        ASH CONTENT

        10.00-14.00%

        ALKALIES

        NIL

        PH

        7-9

        COLOUR

        Faint Black Brown Liquid

        Type of admixture

        Super plasticizer chloride free & IS: 9103

        SP. GRAVITY@27ºC

        1.20 +/- 0.04

        DRY MATERIAL %

        41- 45 %

        CHLORIDE %

        NIL

        ASH CONTENT

        10.00-14.00%

        ALKALIES

        NIL

        PH

        7-9

        COLOUR

        Faint Black Brown Liquid

        TABLE VII. SIEVE ANALYSIS OF 10MM AGGREGATE (IS 383/2386)

    7. Sieve Analysis

      Particle size gradation test are called, sieve analysis. This process used in civil engineering granular material particle size distribution. The particle size distribution by sieve arrangement this type arrangement for particle distribution, called practical size distribution. Sieve arrangement as per IS: 2386 (Part I) 1963. When collect different size partials then sieves arrange standardized by the IS 2386 (Part I) 1963 code.

      1. Fine Aggregate Grading

        • Codes is recommended IS-383:1970.

        • Sand type Banas Sand zone – II.

        • The Sieves arrangement 10mm, 4.75mm, 2.36mm, 1.18mm, 600 micron, 300 micron and 150 micron.

          TABLE VI. SIEVE ANALYSIS FOR SAND (IS 383/2386)

          Sieve size

          Retained (gm)

          %

          Retai ned weigh t

          Cumu lative

          %

          Retai ned

          Cumu lative

          %

          Passin g

          Limit as per IS 383

          Sample 1

          Sam ple 2

          Aver age

          10

          mm

          0

          0

          0

          0

          0

          100

          100

          4.75

          mm

          11.6

          11.5

          11.5

          5

          1.155

          1.15

          98.85

          90-100

          2.36

          mm

          17

          18

          17.5

          1.75

          2.9

          97.1

          75-100

          1.18

          mm

          71

          76

          73.5

          7.35

          10.25

          89.95

          55-90

          600

          micro n

          517.4

          497

          507.

          5

          50.72

          61

          39

          35-59

          300

          micro n

          280

          351

          315.

          5

          31.55

          92.5

          7.5

          8.0-30

          150

          micro n

          991

          41

          66

          6.6

          99.1

          0.9

          0-10

          PAN

          12

          5.5

          8.75

          0.875

          266.9

          Total

          1000

          1000

          1000

          100

          Fineness Modulus = 266.9/100 = 2.66 Grading Zone = II

      2. Coarse Aggregate Grading (10mm)

        • Codes are recommended IS-383:1970.

        • Aggregate type hathipura Aggregate.

        • The Sieves arrangement 12.5mm, 10mm, 4.75mm and 2.36mm.

      0

      Siev e size

      Retained (gm)

      %

      Retain ed weigh t

      Cumu lative

      %

      Retain ed

      Cumu lative

      %

      Passin g

      Limi t as per IS 383

      Samp le 1

      Sampl e 2

      Avera ge

      12.5

      mm

      0

      0

      0

      0

      100

      100

      10

      mm

      38

      42

      40

      2

      2

      98

      85-

      100

      4.75

      mm

      1362

      1360

      1361

      68.05

      70.05

      29.95

      0-20

      2.36

      mm

      493

      492

      492.5

      24.62

      94.67

      5.33

      0-5

      1.18

      mm

      107

      106

      106.5

      5.325

      100

      0

      600

      micr on

      0

      0

      0

      0

      100

      0

      300

      micr on

      0

      0

      0

      0

      100

      0

      150

      micr on

      0

      0

      0

      0

      100

      0

      PAN

      0

      0

      0

      0

      566.7

      2

      Total

      2000

      2000

      2000

      100.0

      0

      Siev e size

      Retained (gm)

      %

      Retain ed weigh t

      Cumu lative

      %

      Retain ed

      Cumu lative

      %

      Passin g

      Limi t as per IS 383

      Samp le 1

      Sampl e 2

      Avera ge

      12.5

      mm

      0

      0

      0

      0

      0

      100

      100

      10

      mm

      38

      42

      40

      2

      2

      98

      85-

      100

      4.75

      mm

      1362

      1360

      1361

      68.05

      70.05

      29.95

      0-20

      2.36

      mm

      493

      492

      492.5

      24.62

      94.67

      5.33

      0-5

      1.18

      mm

      107

      106

      106.5

      5.325

      100

      0

      600

      micr on

      0

      0

      0

      0

      100

      0

      300

      micr on

      0

      0

      0

      0

      100

      0

      150

      micr on

      0

      0

      0

      0

      100

      0

      PAN

      0

      0

      0

      0

      566.7

      2

      Total

      2000

      2000

      2000

      100.0

      0

      Fineness Modulus = 566.72/100 = 5.66

      TABLE VIII. SIEVE ANALYSIS OF 20MM AGGREGATE (IS 383/2386)

      Siev e size

      Retained (gm)

      %

      Retain ed weight

      Cumul ative

      %

      Retain ed

      Cumul ative

      %

      Passin g

      Limit as per IS 383

      Sampl e 1

      Sampl e 2

      Avera ge

      40

      mm

      0

      0

      0

      0

      0

      100

      100

      20

      mm

      1182

      1169

      1175.5

      58.77

      58.80

      41.2

      85-

      100

      10

      mm

      730

      740

      735

      36.75

      95.55

      4.45

      0-20

      4.75

      mm

      70

      90

      80

      4

      99.55

      0.45

      0-5

      2.36

      mm

      18

      1

      9.5

      0.47

      100

      0

      1.18

      mm

      0

      0

      0

      0

      100

      0

      600

      micr on

      0

      0

      0

      0

      100

      0

      300

      micr on

      0

      0

      0

      0

      100

      0

      150

      micr on

      0

      0

      0

      0

      100

      0

      PAN

      0

      0

      0

      0

      757.9

      Total

      2000

      2000

      2000

      100

      Fineness Modulus = 757.9/100 = 7.57

    8. Proportion Mix

      Counting water, coarse aggregate, fine aggregate and cement in specific quantity which required to proper mixing ratio, this type mix called proportion mix. Proper mixing ratio uses for trial mix, control mix and conrtrol mix some variation with GGBS in this experimental work are given below.

    9. Trial Mix

      Which concrete mix prepare by coarse aggregate, fine aggregate, water and cement in ordinary ratio and provide exect strength of concrete as per IS 456:2000, this type mix called trial mix. In this experimental work prepared four trial mix without using admixture.

    10. Control Mix

      As per IS 10262:2009 suggestion and condition Control mix was designed which are given below

      TABLE IX. CONTROL MIX PROPORTION FOR M35 WITH 125MM SLUMP

      S.No.

      Materials

      Weight(Kg)

      1

      Cement(PPC-43)

      404

      2

      Coarse Aggregate(20mm)

      693.00

      3

      Coarse Aggregate(10mm)

      461.44

      4

      Fine Aggregate

      702.24

      5

      Water

      162

      6

      Admixture @ 1.2% of cement

      4.8

      7

      W/C Ratio

      0.40

      TABLE X. CONTROL MIX PROPORTION FOR M40 WITH 135MM SLUMP

      S.No.

      Materials

      Weight(Kg)

      1

      Cement(PPC-43)

      453

      2

      Coarse Aggregate(20mm)

      683.72

      3

      Coarse Aggregate(10mm)

      455.81

      4

      Fine Aggregate

      664.00

      5

      Water

      167.45

      6

      Admixture @ 1.6% of cement

      7.24

      7

      W/C Ratio

      0.37

    11. Proportion of Mineral admixture in Control Mix

    In control mix, cement has two difference variations with GGBS. First difference addition 0% to 25% GGBS of the weight of cement at interval of 5% concrete mixes for M35 & M40 and second difference partial replacement 0% to 25% GGBS of the weight of cement at interval of 5% concrete mixes for M35 & M40.

    TABLE XI. MICRO FINE GGBS ADDITION INTO PPC FOR M35 GRADE

    S.N

    o

    Mix Name

    cemen t (Kg)

    GGBS (Kg)

    Coarse Aggregate(K g)

    Fine Aggregate (Kg)

    Wat er (Kg)

    Admixture (Kg)

    20m m

    10m m

    1

    PPC

    +GGBS (100+0)

    404

    0.00

    693

    461.4

    4

    702.

    24

    161.

    6

    4.8

    2

    PPC

    +GGBS (100+5)

    404

    20.2

    685.

    83

    457.2

    2

    692.

    20

    161.

    6

    4.8

    3

    PPC

    +GGBS (100+10

    )

    404

    40.4

    679.

    80

    453.2

    689.

    19

    161.

    6

    4.8

    4

    PPC

    +GGBS (100+15

    )

    404

    60.6

    672.

    87

    448.5

    8

    682.

    17

    161.

    6

    4.8

    5

    PPC

    +GGBS (100+20

    )

    404

    80.8

    665.

    94

    443.9

    6

    675.

    15

    161.

    6

    4.8

    6

    PPC

    +GGBS (100+25

    )

    404

    101

    659.

    02

    439.3

    4

    668.

    15

    161.

    6

    4.8

    Aggregate

    Aggregate

    (Kg)

    (Kg)

    TABLE XII. REPLACEMENT OF MICRO FINE GGBS INTO PPC FOR M35 GRADE

    S

    . N

    o

    Mix Name

    cemen t (Kg)

    GGBS (Kg)

    Coarse Aggregate(Kg)

    Fine

    (Kg)

    Water (Kg)

    Admixture

    20m m

    10m m

    1

    PPC

    +GGBS (100+0)

    404

    0.00

    693

    461.4

    4

    702.2

    4

    161.6

    4.8

    2

    PPC

    +GGBS (95+5)

    383.8

    20.2

    693.5

    5

    462.3

    6

    702.2

    4

    161.6

    4.8

    3

    PPC

    +GGBS (90+10)

    363.6

    40.4

    689.6

    9

    459.7

    9

    699.2

    3

    161.6

    4.8

    4

    PPC

    +GGBS (85+15)

    343.4

    60.6

    688.7

    0

    459.1

    3

    698.2

    2

    161.6

    4.8

    5

    PPC

    +GGBS (80+20)

    323.2

    80.8

    688.7

    0

    459.1

    3

    698.2

    2

    161.6

    4.8

    6

    PPC

    +GGBS (75+25)

    303

    101

    688.0

    1

    458.6

    7

    697.5

    2

    161.6

    4.8

    S.

    No

    Mix Name

    cem ent (Kg)

    GGBS (Kg)

    Coarse Aggregate(Kg)

    Fine Aggregate (Kg)

    Wat er (Kg)

    Admixture (Kg)

    20m m

    10mm

    1

    PPC

    +GGBS (100+0)

    453

    0

    683.

    72

    455.61

    664

    167.

    45

    7.24

    2

    PPC

    +GGBS (100+5)

    453

    22.6

    5

    676.

    68

    451.12

    657.

    38

    167.

    45

    7.24

    3

    PPC

    +GGBS (100+10

    )

    453

    45.3

    688.

    04

    445.36

    648.

    59

    167.

    45

    7.24

    4

    PPC

    +GGBS (100+15

    )

    453

    67.9

    5

    660.

    60

    440.4

    641.

    75

    167.

    45

    7.24

    5

    PPC

    +GGBS (100+20

    )

    453

    90.5

    6

    652.

    55

    435.03

    633.

    94

    167.

    45

    7.24

    6

    PPC

    +GGBS (100+25

    )

    453

    113.

    19

    644.

    51

    429.67

    626.

    12

    167.

    45

    7.24

    S.

    No

    Mix Name

    cem ent (Kg)

    GGBS (Kg)

    Coarse Aggregate(Kg)

    Fine Aggregate (Kg)

    Wat er (Kg)

    Admixture (Kg)

    20m m

    10mm

    1

    PPC

    +GGBS (100+0)

    453

    0

    683.

    72

    455.61

    664

    167.

    45

    7.24

    2

    PPC

    +GGBS (100+5)

    453

    22.6

    5

    676.

    68

    451.12

    657.

    38

    167.

    45

    7.24

    3

    PPC

    +GGBS (100+10

    )

    453

    45.3

    688.

    04

    445.36

    648.

    59

    167.

    45

    7.24

    4

    PPC

    +GGBS (100+15

    )

    453

    67.9

    5

    660.

    60

    440.4

    641.

    75

    167.

    45

    7.24

    5

    PPC

    +GGBS (100+20

    )

    453

    90.5

    6

    652.

    55

    435.03

    633.

    94

    167.

    45

    7.24

    6

    PPC

    +GGBS (100+25

    )

    453

    113.

    19

    644.

    51

    429.67

    626.

    12

    167.

    45

    7.24

    TABLE XIII. MICRO FINE GGBS ADDITION INTO PPC FOR M40 GRADE

    (Kg)

    (Kg)

    TABLE XIV. REPLACEMENT OF PPC BY MICRO FINE GGBS FOR M40 GRADE

    to 25% interval 5% and second partial replacement of cement by GGBS material 5% to 25% interval 5%. This type variation same all cube specimen, cylinder specimen and beam specimen for find out the density, compressive strength, split tensile strength and flexural strength of M35 & M40 grade concrete.

    B. Workability Test Result

    Slump increased and decrease by addition and partial replacement of mineral admixtures such as Micro fine GGBS material. The workability has been used to improve placing of concrete, flexibility, compatibility and finishing capacity. Slump can be increased by addition of chemical admixtures such as plasticizer or super plasticizer without changing the water-cement ratio. Some other admixtures, especially air- entraining admixture, can raise the slump of concrete mix.

    Concrete mix designs source 125 mm slump for M35 and 135 mm slump for M40 grade concrete. Graphs are given as result find out

    S.No

    Percentage of GGBS

    Addition (mm)

    Replacement (mm)

    1

    0

    125

    125

    2

    5

    154

    137

    3

    10

    146

    152

    4

    15

    138

    156

    5

    20

    132

    161

    6

    25

    128

    164

    S.No

    Percentage of GGBS

    Addition (mm)

    Replacement (mm)

    1

    0

    125

    125

    2

    5

    154

    137

    3

    10

    146

    152

    4

    15

    138

    156

    5

    20

    132

    161

    6

    25

    128

    164

    TABLE XV. COMPARISON OF SLUMP ON ADDITION & REPLACEMENT FOR M35 GRADE

    S

    . N

    o

    Mix Name

    ceme nt (Kg)

    GGBS

    Coarse Aggregate(Kg)

    Fine Aggregate

    Water (Kg)

    Admixture (Kg)

    20m m

    10mm

    1

    PPC

    +GGB S (100+0)

    452.5

    6

    0

    683.

    72

    455.6

    1

    664

    167.45

    7.24

    2

    PPC

    +GGB S (95+5)

    429.9

    4

    22.

    65

    684.

    73

    456.4

    8

    665

    .2

    167.45

    7.24

    3

    PPC

    +GGB S (90+10)

    407.3

    1

    45.

    3

    684.

    12

    456.0

    8

    664

    .22

    167.45

    7.24

    4

    PPC

    +GGB S (85+15)

    384.6

    8

    67.

    95

    683.

    72

    455.8

    1

    664

    .22

    167.45

    7.24

    5

    PPC

    +GGB S (80+20)

    362.0

    5

    90.

    56

    683.

    72

    455.8

    1

    664

    .22

    167.45

    7.24

    6

    PPC

    +GGB S (75+25)

    339.4

    2

    113

    .19

    682.

    72

    455.1

    4

    663

    .24

    167.45

    7.24

    S

    . N

    o

    Mix Name

    ceme nt (Kg)

    GGBS

    Coarse Aggregate(Kg)

    Fine Aggregate

    Water (Kg)

    Admixture (Kg)

    20m m

    10mm

    1

    PPC

    +GGB S (100+0)

    452.5

    6

    0

    683.

    72

    455.6

    1

    664

    167.45

    7.24

    2

    PPC

    +GGB S (95+5)

    429.9

    4

    22.

    65

    684.

    73

    456.4

    8

    665

    .2

    167.45

    7.24

    3

    PPC

    +GGB S (90+10)

    407.3

    1

    45.

    3

    684.

    12

    456.0

    8

    664

    .22

    167.45

    7.24

    4

    PPC

    +GGB S (85+15)

    384.6

    8

    67.

    95

    683.

    72

    455.8

    1

    664

    .22

    167.45

    7.24

    5

    PPC

    +GGB S (80+20)

    362.0

    5

    90.

    56

    683.

    72

    455.8

    1

    664

    .22

    167.45

    7.24

    6

    PPC

    +GGB S (75+25)

    339.4

    2

    113

    .19

    682.

    72

    455.1

    4

    663

    .24

    167.45

    7.24

    165

    160

    155

    150

    Slump

    Slump

    145

    140

    135

    130

    125

    Addtion Replacement

  3. RESULTS AND ANALYSIS

    A. Introduction

    In this study find out the M35 & M40 grade specimens result on deferent type variation of GGBS in cement concrete and compare each other and represented it draw by graphs.

    120

    0

    % o1f0GGBS

    20 30

    In this experiment work make different variation specimens of concrete mix. Concrete mix has two type variations, first partial addition of cement by Micro fine GGBS material 5%

    Fig. 1. Influence of Micro fine GGBS on Slump of Concrete (M-35) on

    Addition & Replacement

    TABLE XVI. COMPARISON OF SLUMP ON ADDITION & REPLACEMENT FOR M40 GRADE

    S.No

    Percentage of GGBS

    Addition (mm)

    Replacement (mm)

    1

    0

    135

    135

    2

    5

    160

    145

    3

    10

    146

    158

    4

    15

    138

    160

    5

    20

    130

    162

    6

    25

    126

    169

    170

    170

    160

    160

    2480

    2470

    2460

    2450

    2440

    2430

    2420

    0 5 10 15 20 25

    150

    150

    Addtion

    Addtion

    140

    140

    Slump

    Slump

    % of GGBS

    Addition

    Replace ment

    Replacemen

    t

    Replacemen

    t

    130

    130

    120

    120

    0

    10

    % of GGBS

    20

    30

    0

    10

    % of GGBS

    20

    30

    Fig. 2. Influence of Micro fine GGBS on Slump of Concrete (M-40) on Addition & Replacement

    Fig. 3. Influence of Micro fine GGBS on Density of Hardened Concrete (M-35) on Addition & Replacement

    TABLE XVIII. DENSITY OF HARDENED CONCRETE ON ADDITION OF MICRO FINE GGBS INTO PPC & REPLACEMENT OF PPC BY MICRO FINE GGBS FOR M40 GRADE

    S.No

    Percentage of GGBS

    Density of Hardened Concrete (Kg/m3)

    Addition

    Replacement

    1

    0

    2449.33

    2449.33

    2

    5

    2453.33

    2451.15

    3

    10

    2465.25

    2454.15

    4

    15

    2470.26

    24560.86

    5

    20

    2474.38

    2465.32

    6

    25

    2482.33

    2471.12

    1. Density Test Result

      The specimen of cube, beam & cylinder density was determined before testing. Average weight of Cube, Beam and Cylinder are 8.28Kg (for 7 days)& 8.30 Kg (for 28 days), 12.80Kg ( for 28 days) and 39.35 Kg ( for 28 days) respectively and volume of Cube Beam and Cylinder are 0.003375 meter cube, 0.01575 meter cube and 0.0052 meter cube respectively.

      TABLE XVII. DENSITY OF HARDENED CONCRETE ON ADDITION OF MICRO FINE GGBS INTO PPC & REPLACEMENT OF PPC BY MICRO FINE GGBS FOR M35

      S.No

      Percentage of GGBS

      Density of Hardened Concrete (Kg/m3)

      Addition

      Replacement

      1

      0

      2441.33

      2441.33

      2

      5

      2450.15

      2448.12

      3

      10

      2460.25

      2455.15

      4

      15

      2464.20

      2459.86

      5

      20

      2468.32

      2464.32

      6

      25

      2474.12

      2465.18

      2490

      2480

      2470

      2460

      2450

      2440

      2430

      0 5 10 15 20 25

      % of GGBS

      Addition

      Replace ment

      Fig. 4. Influence of Micro fine GGBS on Density of Hardened Concrete (M-40) on Addition & Replacement

    2. Compressive Strength

      The specimens were cured in water tank for 7 days and 28 days before compressive strength testing after specimens were came out in curing tank and cleaned cotton cloths. Compressive strength of all cube specimens 150mm(length) x 150mm(width) x 150mm(depth) measured as per IS 516:1959.

      TABLE XIX. COMPARISON OF COMPRESSIVE STRENGTH FOR 7 DAYS ON ADDITION & REPLACEMENT FOR M35 GRADE

      S.No

      Percentage of GGBS

      Addition (N/mm2)

      Replacement (N/mm2)

      1

      0

      29.55

      29.55

      2

      5

      31.77

      30.00

      3

      10

      31.91

      31.33

      4

      15

      32.26

      31.33

      5

      20

      32.17

      30.66

      6

      25

      32.22

      31.00

      33

      32

      -5 5

      % of15GGBS

      25

      -5 5

      % of15GGBS

      25

      50

      49

      48

      47

      50

      49

      48

      47

      Addition

      Addition

      46

      45 Replacem

      ent

      44

      43

      42

      41

      46

      45 Replacem

      ent

      44

      43

      42

      41

      Compressive Srength (N/mm2)

      Compressive Srength (N/mm2)

      Fig. 6. Influence of Micro fine GGBS on Concrete of M35 Grade on Addition & Replacement for 28 Days Compressive Strength of Cube

      TABLE XXI. COMPARISON OF COMPRESSIVE STRENGTH FOR 7 DAYS ON ADDITION & REPLACEMENT FOR M40 GRADE

      Compressive Srength

      Compressive Srength

      S.No

      Percentage of GGBS

      Addition (N/mm2)

      Replacement (N/mm2)

      1

      0

      32.66

      32.66

      2

      5

      34.33

      33.55

      3

      10

      35.33

      34.33

      4

      15

      35.60

      34.77

      5

      20

      36.62

      34.44

      6

      25

      36.97

      34.48

      S.No

      Percentage of GGBS

      Addition (N/mm2)

      Replacement (N/mm2)

      1

      0

      32.66

      32.66

      2

      5

      34.33

      33.55

      3

      10

      35.33

      34.33

      4

      15

      35.60

      34.77

      5

      20

      36.62

      34.44

      6

      25

      36.97

      34.48

      31

      Addition Replacement

      30

      37

      37

      Compressive Srength (N/mm2)

      Compressive Srength (N/mm2)

      29

      36

      36

      0 10% of GGBS20 30

      Fig. 5. Influence of Micro fine GGBS on Concrete of M35 Grade on Addition & Replacement for 7 Days Compressive Strength of Cube

      TABLE XX. COMPARISON OF COMPRESSIVE STRENGTH FOR 28 DAYS ON ADDITION & REPLACEMENT FOR M35 GRADE

      S.No

      Percentage of GGBS

      Addition (N/mm2)

      Replacement (N/mm2)

      1

      0

      43.30

      43.30

      2

      5

      45.39

      44.25

      3

      10

      46.26

      44.54

      4

      15

      47.87

      45.14

      5

      20

      48.71

      45.37

      6

      25

      49.54

      45.67

      35

      Addition

      Replacement

      35

      Addition

      Replacement

      34

      34

      33

      33

      32

      -5

      5

      % of GGBS

      25

      32

      -5

      5

      % of GGBS

      25

      15

      15

      Fig. 7. Influence of Micro fine GGBS on Concrete of M40 Grade on Addition & Replacement for 7 Days Compressive Strength of Cube

      S.No

      Percentage of GGBS

      Addition(N/ mm2)

      Replacement(N/mm2)

      1

      0

      48.29

      48.29

      2

      5

      50.75

      48.93

      3

      10

      51.83

      49.79

      4

      15

      53.27

      50.23

      5

      20

      54.31

      50.42

      6

      25

      55.18

      50.69

      S.No

      Percentage of GGBS

      Addition(N/ mm2)

      Replacement(N/mm2)

      1

      0

      48.29

      48.29

      2

      5

      50.75

      48.93

      3

      10

      51.83

      49.79

      4

      15

      53.27

      50.23

      5

      20

      54.31

      50.42

      6

      25

      55.18

      50.69

      TABLE XXII. COMPARISON OF COMPRESSIVE STRENGTH FOR 28 DAYS ON ADDITION & REPLACEMENT FOR M40 GRADE

      Addition & Replacement- M35

      9

      Flexural Strength

      Flexural Strength

      8.5

      8

      7.5

      56

      55

      Compressive Srength

      Compressive Srength

      54

      53 Addi

      tion

      52

      7

      6.5

      6

      5.5

      5

      -5

      Addition Replacement

      %5 of GGBS15 25

      51

      50

      49

      48

      % of GGBS

      0 5 10 15

      20 25

      Fig. 9. Influence of Micro fine GGBS on Concrete of M35 Grade on Addition & Replacement for 28 Days Flexural Strength of Beam

      TABLE XXIV. COMPARISON OF FLEXURAL STRENGTH FOR 28 DAYS ON ADDITION & REPLACEMENT FOR M40 GRADE

      S.No

      Percentage of GGBS

      Addition(N/mm2)

      Replacement(N/mm2)

      1

      0

      6.85

      6.85

      2

      5

      8.55

      7.47

      3

      10

      9.2

      7.83

      4

      15

      9.52

      8.03

      5

      20

      9.74

      8.72

      6

      25

      9.61

      8.41

      S.No

      Percentage of GGBS

      Addition(N/mm2)

      Replacement(N/mm2)

      1

      0

      6.85

      6.85

      2

      5

      8.55

      7.47

      3

      10

      9.2

      7.83

      4

      15

      9.52

      8.03

      5

      20

      9.74

      8.72

      6

      25

      9.61

      8.41

      Fig. 8. Influence of Micro fine GGBS on Concrete of M40 Grade on Addition & Replacement for 28 Days Compressive Strength of Cube

    3. Flexural Strength:

      The specimens were cured in water tank for 28 days before flexural strength testing after specimens were came out in curing tank and cleaned cotton cloths. The central point loading method was applied for this testing. flexural strength of all beam specimens 700mm(length) x 150mm(width) x 150mm(depth) measured as per IS 516:1959.

      TABLE XXIII. COMPARISON OF FLEXURAL STRENGTH FOR 28 DAYS ON ADDITION & REPLACEMENT FOR M35 GRADE

      Addition & Replacement- M40

      Flexural Strength (N/mm2)

      Flexural Strength (N/mm2)

      10

      9.5

      9

      8.5

      S.No

      Percentage of GGBS

      Addition (N/mm2)

      Replacement (N/mm2)

      1

      0

      5.96

      5.96

      2

      5

      7.47

      6.58

      3

      10

      7.83

      6.76

      4

      15

      7.92

      7.12

      5

      20

      8.36

      7.29

      6

      25

      8.01

      6.85

      S.No

      Percentage of GGBS

      Addition (N/mm2)

      Replacement (N/mm2)

      1

      0

      5.96

      5.96

      2

      5

      7.47

      6.58

      3

      10

      7.83

      6.76

      4

      15

      7.92

      7.12

      5

      20

      8.36

      7.29

      6

      25

      8.01

      6.85

      8

      7.5

      7

      6.5

      6

      Addition Replacement

      % of GGBS

      0 5 10 15 20 25

      Fig. 10. Influence of Micro fine GGBS on Concrete of M40 Grade on Addition & Replacement for 28 Days Flexural Strength of Beam

    4. Splitting Tensile Strength

    The specimens were cured in water tank for 28 days before split tensile strength testing after specimens were came out in curing tank and cleaned cotton cloths. split tensile strength of all cylinder specimens 300mm (length) x 150mm (diameter) measured as per IS 516:1959.

    TABLE XXV. COMPARISON OF SPLITTING TENSILE STRENGTH FOR 28 DAYS ON ADDITION & REPLACEMENT FOR M35 GRADE

    S.No

    Percentage of GGBS

    Addition (N/mm2)

    Replacement (N/mm2)

    1

    0

    2.70

    2.70

    2

    5

    2.95

    2.89

    3

    10

    3.20

    2.97

    4

    15

    3.28

    3.02

    5

    20

    3.35

    3.20

    6

    25

    3.38

    3.31

    3.9

    3.7

    3.5

    3.3

    3.1

    Addition & Replacement – M40

    Addition Replacement

    Addition & Replacement- M35

    3.4

    3.2

    3

    Addition & Replacement- M35

    3.4

    3.2

    3

    Spilting Tensile Strength (N/mm2)

    Spilting Tensile Strength (N/mm2)

    2.9

    (N/mm2)

    (N/mm2)

    -5 5 % of GGB1S5 25

    Tensile Strength

    Tensile Strength

    Fig. 12. Influence of Micro fine GGBS on Concrete of M40 Grade on Addition & Replacement for 28 Days Splitting Tensile Strength of Cylinder

    2.8

    2.6

    Addition

    Replacement

    Spilting

    Spilting

    2.8

    2.6

    Addition

    Replacement

    2.4

    2.2

    % of GGBS

    2.4

    2.2

    % of GGBS

    -5

    5

    15

    25

    -5

    5

    15

    25

    2

    2

    Fig. 11. Influence of Micro fine GGBS on Concrete of M35 Grade on Addition & Replacement for 28 Days Splitting Tensile Strength of Cylinder

    TABLE XXVI. COMPARISON OF SPLITTING TENSILE STRENGTH FOR 28 DAYS ON ADDITION & REPLACEMENT FOR M40 GRADE

    S.No

    Percentage of GGBS

    Addition(N/mm2

    )

    Replacement(N/mm2)

    1

    0

    2.97

    2.97

    2

    5

    3.61

    3.30

    3

    10

    3.65

    3.54

    4

    15

    3.76

    3.68

    5

    20

    3.80

    3.78

    6

    25

    3.90

    3.73

  4. CONCLUSIONS

  1. Evaluate the results of Slump by fresh concrete, it give conclusions

    • Concrete mix slump was decreased with addition of Micro fine GGBS in PPC, because number of fine particle increased or surface area increased than concrete mix water demand increased. Slump on 25% addition of Micro fine GGBS in PPC was closed to the control mix concrete slump.

    • Concrete mix slump was increased with partial replacement of Micro fine GGBS in PPC, because cement replaced by micro fine GGBS than concrete mix water demand decreased. Partial replacement of Micro fine GGBS in PPC Slump was increased at all percentage interval compare to the control mix concrete slump.

    • 154mm slump was found addition of 5% micro fine GGBS into PPC & 152mm slump was found partial replacement of 10% micro fine GGBS into PPC for M35 grade. 164mm high slump was found partial replacement 25% micro fine GGBS into PPC for M35 grade.

    • 160mm slump was found addition of 5% micro fine GGBS into PPC & 160mm slump was found partial replacement of 15% micro fine GGBS into PPC for M40 grade. 169mm high slump was found partial replacement 25% micro fine GGBS into PPC for M40 grade.

  2. Evaluate the results of density by hardened concrete specimens, it give conclusions

    • Control mix for M35 & M40 grade concrete specimens density was lower compare to M35 & M40 grade concrete specimens with addition & partial replacement of Micro fine GGBS in PPC. Addition and replacement of Micro fine GGBS in PPC for grade M35 & M40 was make a packing material, there internal system develops gel pores, which are smaller than the normal concrete pores of PPC, So compressive strength, flexural strength, Splitting tensile strength greater compare to normal concrete compressive strength, flexural strength, Splitting tensile strength.

  3. Evaluate the results of compressive Strength by cube specimens, it give conclusions

    • Concrete compressive strength was greater in addition of Micro fine GGBS in PPC compare to partial replacement of Micro fine GGBS in PPC. The compressive strength addition and replacement greater than control mix concrete for M35 & M40 grade.

    • The maximum compressive strength 49.54 N/mm2 was found addition of Micro fine GGBS in PPC for M35 grade, this compressive strength was 14.41% greater than compare to M35 grade control mix concrete. Similarly maximum compressive strength 55.18 N/mm2 was found addition of Micro fine GGBS in PPC for M40 grade, this compressive strength was 14.26% greater than compare to M40 grade control mix concrete.

    • 48.71 N/mm2 compressive strength was found addition 20% micro fine GGBS into PPC for grade M35; it was equal to the target value of M40 grade concrete. Similarly 53.27N/mm2 compressive strength was found addition 15% micro fine GGBS into PPC for grade M40; it was equal to the target value of M45 grade concrete.

  4. Evaluate the results of flexural Strength by beam specimens

    • Concrete Flexural strength was greater in addition of Micro fine GGBS in PPC compare to partial replacement of Micro fine GGBS in PPC. Flexural strength in addition was greater than control mix concrete of M35 & M40 grade.

    • The maximum flexural strength 8.36N/mm2 was found addition 20% Micro fine GGBS in PPC for M35 grade, this flexural strength was 40.26% greater than compare to M35 grade control mix concrete. Similarly maximum flexural strength 9.74N/mm2 was found addition 20% Micro fine GGBS in PPC for M40 grade, this flexural strength was 42.18% greater than compare to M40 grade control mix concrete.

  5. Evaluate the results of split Tensile Strength by cylinder, it give conclusions

    • Concrete Split tensile strength was greater in addition of Micro fine GGBS in PPC compare to partial replacement of Micro fine GGBS in PPC. Splitting tensile strength in

      addition was greater than control mix concrete of M35 & M40 grade.

    • The maximum Split tensile strength 3.38N/mm2 was found addition 25% Micro fine GGBS in PPC for M35 grade, this Split tensile strength was 25.18% greater than compare to M35 grade control mix concrete. Similarly maximum Split tensile strength 3.90 N/mm2 was found addition 25% Micro fine GGBS in PPC for M40 grade, this Split tensile strength was 31.31% greater than compare to M40 grade control mix concrete.

    REFERENCES

    1. Sonali K. Gadpalliwar, R. S. Deotale, Abhijeet R.Narde, To Study the Partial Replacement of Cement by GGBS & RHA and Natural Sand by Quarry Sand In Concrete IOSR Journal of Mechanical and Civil Engineering (IOSR-JMCE), Volume 11, Issue 2 ,PP 69-77, (Mar- Apr. 2014),

    2. Siddharth P. Upadhyay, M. A. Jamnu Effect on Compressive strength of High Performance Concrete Incorporating Alccofine and Fly Ash. International Journal of Innovative Research & Development, volume 3, issue 2, pp 124-128, February 2014.

    3. S. Arivalagan,Sustainable Studies on Concrete with GGBS As a Replacement Material in Cement Jordan Journal of Civil Engineering, Volume 8, No.3, 2014.

    4. Mo.Tofik Y. Patel, Siddharth P Upadhyay, Prof. A.R. Darji, Prof.

      M.A. Jamnu To Study on Effect of High Performance Concrete with Alccofine and Waste Glass Powder. International Journal for Scientific Research & Development ISSN 2321-0613, Vol. 2, Issue 04, 2014.

    5. Yogendra O. Patil, Prof.P.N.Patil, Dr.Arun Kumar Dwivedi, GGBS as Partial Replacement of OPC in Cement Concrete An Experimental Study International Journal for Scientific Research & Development, ISSN No 2277 – 8179, Volume : 2,November 2013.

    6. Abhijit singh Parmar, Dhaval Patel Experimental study on high performance concrete by using alccofine and fly ash. International journal of pure and applied research in engineering and technology 2013,ISSN 2319-507volume 2(5),Published Date: 01/01/2014

    7. P. J. Patel and H. S. Patel (2013) High performance concrete with alccofine and fly ash.OPC-53 grade cement replacement by partial of alccofine and fly ash. International Journal of Civil, Structural, Environmental and Infrastructure Engineering, Research and Development (IJCSEIERD),ISSN 2249-6866, Vol. 3, Issue 2, 2013,

    8. IS 1199:1959, Methods of sampling and analysis of concrete, Bureau of Indian Standards, New Delhi.

    9. IS 2386:1963, Methods of test for aggregates for concrete, Bureau of Indian Standards, New Delhi.

    10. IS 383:1970, Specification for coarse and fine aggregates from natural sources for concrete, Bureau of IndianStandards, New Delhi.

    11. IS 456:2000, "Plain and Reinforced Concrete Code of Practice", Bureau of Indian Standards, New Delhi.

    12. IS 516:1959, 'METHODS OF TESTS FOR STRENGTH OF

CONCRETE., BUREAU OF INDIAN STANDARDS

Leave a Reply